Lightweight carbon-ceramic integrated heat-insulating material with SiC ceramic layer and its preparation

By generating a nanowire-toughened gradient SiC coating on the surface of a lightweight carbon-based composite material, the oxidation problem of the lightweight carbon-based composite material in a high-temperature and oxygen-containing environment is solved, realizing a lightweight carbon-ceramic composite material that integrates heat protection, heat insulation, and load-bearing capacity, and has excellent anti-oxidation and heat insulation properties.

CN119100845BActive Publication Date: 2026-11-17INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411220429.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2026-11-17
Estimated Expiration
2044-09-02

Smart Images

  • Figure CN119100845B_ABST
    Figure CN119100845B_ABST
Patent Text Reader

Abstract

This invention discloses a lightweight carbon-ceramic integrated thermal insulation material and its preparation method, belonging to the technical field of ultra-high temperature thermal protection materials. This invention employs a nanopowder-induced SiC nanowire synergistic low-temperature gas-solid reaction ceramicization technology. By setting a nanowire growth induction layer containing nano-ceramic powder on the surface of a lightweight carbon-based composite material, SiC nanowires are induced to form under low-temperature silicon-carbon gas-solid reaction, thus achieving ceramicization of the surface layer of the lightweight carbon-based composite material. The resulting material has a surface layer of 100–800 μm SiC nanowire-toughened gradient SiC ceramic layer, which provides ultra-high temperature oxidation and ablation resistance. The bottom layer is an unreacted lightweight carbon-based composite material substrate, which provides ultra-high temperature thermal insulation and load-bearing functions, thereby achieving an integrated ultra-high temperature non-ablation thermal insulation and load-bearing structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ultra-high temperature thermal protection materials technology, specifically to a lightweight carbon-ceramic composite material integrating heat protection, heat insulation, and load bearing, and its preparation method. Background Technology

[0002] Novel lightweight carbon-based composite materials are a class of porous carbon materials made with a three-dimensional carbon network as the matrix and carbon fibers as the reinforcement. They possess very low density and a porosity as high as 80%-99%, making them highly promising for thermal protection applications in aerospace vehicles and their propulsion systems. However, both the carbon matrix and carbon fibers are highly susceptible to oxidation above 400°C, and their porous structure results in a faster oxidation rate than traditional graphite and carbon / carbon composites, which significantly limits their application in high-temperature, oxygen-containing environments. Preparing an antioxidant coating on the material surface can significantly improve its antioxidant properties, potentially driving the application of novel lightweight carbon-based composite materials in the field of thermal protection.

[0003] Ceramic coatings, characterized by their dense structure and low oxygen permeability, have been extensively studied as antioxidant coatings for carbon-based composites. However, due to the inherent brittleness of ceramic coatings and the significant mismatch in structure and elastic modulus between the ceramic and the porous carbon matrix, the resulting ceramic coatings are prone to cracking. Therefore, preparing ceramic coatings with high fracture toughness is crucial for ensuring antioxidant performance.

[0004] Therefore, this invention employs a nanopowder-induced SiC nanowire synergistic low-temperature gas-solid reaction ceramicization technology. By setting a nanowire growth induction layer containing nano-ceramic powder on the surface of a lightweight carbon-based composite material, SiC nanowires are induced to form under low-temperature silicon-carbon gas-solid reaction, thereby realizing the ceramicization transformation of the surface layer of the lightweight carbon-based composite material from carbon to ceramic. Finally, a nanowire-toughened and antioxidant coating is prepared on the surface of the lightweight carbon-based composite material, providing reliable oxidation protection for the carbon substrate. Summary of the Invention

[0005] The purpose of this invention is to provide a novel method for preparing a nanowire-toughened gradient SiC coating on the surface of a lightweight carbon-based composite material, so as to obtain a lightweight carbon-ceramic composite material that integrates heat protection, heat insulation, and load bearing, thereby meeting the thermal protection requirements in ultra-high temperature and oxygen-containing environments.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] A novel method for preparing a nanowire-toughened gradient SiC coating on the surface of a lightweight carbon-based composite material includes the following steps:

[0008] (1) With a density of 0.2~0.8g / cm³ 3 The lightweight carbon-based composite material is used as the base, processed into the required shape, ultrasonically cleaned with alcohol, and then dried in an oven at 80-120℃ for 24-48 hours before use.

[0009] (2) Weigh a certain amount of nanoparticles, dispersant (polyethyleneimine, PEI), and deionized water into a beaker, place it on a magnetic stirrer and stir for 5 to 10 hours until the ceramic powder is dispersed in the deionized water; transfer the above solid-liquid mixture into a ball mill jar and ball mill for 3 to 5 hours (ball milling avoids agglomeration of nanoparticles) to obtain nano-ceramic powder slurry.

[0010] (3) Immerse the lightweight carbon-based composite material substrate completely in the nano-ceramic powder slurry, dip it in the slurry for 3-5 seconds, take it out, dry the surface at 80-120℃, and then immerse it in the slurry again. Repeat the above operation until the substrate surface is covered with enough nano-ceramic powder.

[0011] (4) After sieving boron carbide (B4C), silicon carbide (SiC), silicon dioxide (SiO2), aluminum oxide (Al2O3) and boron trioxide (B2O3) micron powder (particle size 3-5μm), weigh them according to 25wt.% boron carbide, 25wt.% silicon carbide, 15wt.% silicon dioxide, 15wt.% aluminum oxide and 20wt.% boron trioxide, and then ball-mill them with alcohol (the above powders have large differences in density, and ordinary dry mixing is prone to uneven stratification. Using alcohol wet ball milling can obtain a more uniform powder slurry) for 8-10 hours to obtain micron powder slurry.

[0012] (5) Apply the micron powder slurry obtained in step (4) to the surface of the lightweight carbon-based composite material substrate with nanoparticles obtained in step (3) using a brushing process. After air drying, dry it at 100-130℃ for 2-5 hours for later use.

[0013] (6) Sprinkle a certain amount of high-purity silicon powder evenly around the bottom of the graphite crucible, place the substrate material dried in step (5) on top of the silicon powder, and place it in a high-temperature furnace for high-temperature treatment: raise the temperature from room temperature to 1300-1600℃ at a rate of 5-10℃ / min, keep it at the target temperature for 1-5 hours, and then cool it to room temperature to remove the sample. Finally, a SiC nanowire toughened gradient SiC ceramic layer is obtained in situ on the surface of the lightweight carbon-based composite material, thus realizing the preparation of a lightweight carbon-ceramic heat insulation integrated material.

[0014] In step (2) above, the types and contents of nano-ceramic powders include, but are not limited to, one of the following three types:

[0015] (1) Nano-ceramic powder 1: ZrO2 powder 10-20 wt.%, C powder 30-50 wt.%, SiO2 powder 30-50 wt.%;

[0016] (2) Nano-ceramic powder 2: ZrO2 powder 10-30 wt.%, C powder 40-60 wt.%, Al2O3 powder 20-50 wt.%;

[0017] (3) Nano-ceramic powder 3: Al2O3 powder 20-30 wt.%, C powder 30-40 wt.%, SiO2 powder 40-50 wt.%.

[0018] The lightweight carbon-ceramic heat-insulating integrated material prepared by this invention has a surface layer of 100-800μm SiC nanowire-toughened gradient SiC ceramic layer, which plays a role in ultra-high temperature oxidation resistance and ablation resistance. The bottom layer is an unreacted lightweight carbon-based composite material substrate, which plays a role in ultra-high temperature heat insulation and load-bearing, thereby realizing the integration of ultra-high temperature non-ablation heat insulation and load-bearing.

[0019] The design mechanism of this invention is as follows:

[0020] This invention, without the need for an iron-nickel catalyst, utilizes nano-oxide powder to induce nanowire growth, generating a large number of SiC nanowires on the material surface. Simultaneously, it relies on the in-situ synthesis of a gradient SiC ceramic layer through the reaction of gaseous silicon with a carbon matrix, hindering oxygen diffusion into the carbon substrate and thus endowing the carbon material with antioxidant properties. The principle is that some carbon in the nanowire-induced layer reacts with nanoscale SiO2, ZrO2, or Al2O3 to generate CO intermediates. The intermediate CO reacts with Si vapor to form SiC nuclei, which then accumulate according to the principle of minimum energy to form nanowires. Simultaneously, some silicon vapor reacts directly with carbon particles in the induced layer to generate SiC particles; and some silicon diffuses into the carbon matrix, causing it to ceramize and form the SiC ceramic layer.

[0021] The present invention has the following beneficial effects:

[0022] 1. The method described in this invention does not require a separate nanowire growth process; nanowires can be generated simultaneously during the ceramization process, which has the significant advantage of simple process.

[0023] 2. The method described in this invention does not require the addition of catalysts such as ferric nitrate or nickel nitrate to induce nanowire growth, effectively avoiding the adverse effects of additives on the antioxidant properties of the coating. Attached Figure Description

[0024] Figure 1 The cross-sectional microstructure of the lightweight carbon-ceramic material with coating in Example 1 is shown in the following figures: (a) coating thickness, (b) magnified view of the outer coating structure showing the morphology of the nanowires, and (c) microstructure of the porous carbon matrix.

[0025] Figure 2 The microstructure of the lightweight carbon-ceramic material with coating in Example 1 after 10 thermal shocks at room temperature to 1700°C;

[0026] Figure 3The macroscopic morphology and cross-sectional microstructure of the coated lightweight carbon-ceramic material in Example 1 after oxyacetylene ablation at 1700℃ for 300s are shown.

[0027] Figure 4 The temperature change curves of the ablation surface and the ablation back side of the 10mm thick lightweight carbon-ceramic material in Example 1 during the oxyacetylene ablation process at 1700℃ are shown over time.

[0028] Figure 5 The microstructure of the lightweight carbon-ceramic cross section with coating in Example 2 is shown in the following figures: (a) coating thickness, (b) magnified view of the outer coating structure showing the morphology of the nanowires, and (c) microstructure of the porous carbon matrix.

[0029] Figure 6 The microstructure of the coated lightweight carbon-ceramic material in Example 2 after 10 thermal shocks at room temperature to 1700°C;

[0030] Figure 7 The surface microstructure of the coated lightweight carbon-ceramic material in Example 2 after oxyacetylene ablation at 1700°C for 300s.

[0031] Figure 8 The temperature change curves over time of the ablation surface and the ablation back side of the 10mm thick lightweight carbon-ceramic material in Example 2 during the oxyacetylene ablation process at 1700℃.

[0032] Figure 9 The cross-sectional microstructure of the coating obtained without the nanowire induction layer in Comparative Example 1 is shown in (a) microstructure of the coating and substrate, and (b) magnified view of the outer coating structure, in which no nanowire distribution is observed. Detailed Implementation

[0033] To further understand the present invention, the following description, in conjunction with examples, illustrates the low-temperature gas-solid reaction ceramicization technology of SiC nanowires induced by nanopowder. However, these examples are merely for further elaboration of the features and advantages of the present invention and are not intended to limit the scope of the claims of the present invention.

[0034] Example 1

[0035] (1) With a density of 0.6 g / cm³ 3 Using lightweight carbon-based composite material (C / CA, Institute of Metal Research, Chinese Academy of Sciences) as the substrate, the material was processed into a cylinder with a diameter of 30 mm and a thickness of 10 mm. After ultrasonic cleaning with alcohol, the cylinder was dried in an oven at 100°C for 24 hours before use.

[0036] (2) Weigh out the following nano-ceramic powders according to the following mass ratio: 20 wt.% ZrO2 powder, 50 wt.% C powder, and 30 wt.% SiO2 powder. Mix the above nano-ceramic powders with dispersant (polyethyleneimine, PEI) and deionized water in a mass ratio of 2:1:1 and stir on a magnetic stirrer for 8 hours until the ceramic powders are uniformly dispersed in the deionized water. Transfer the above solid-liquid mixture into a ball mill jar and ball mill for 5 hours to obtain a nano-ceramic powder slurry.

[0037] (3) The lightweight carbon-based composite material substrate is completely immersed in the nano-ceramic powder slurry. After dipping in the slurry for 5 seconds, it is taken out and dried at 100°C. The above immersion, dipping and drying operations are repeated twice until the substrate surface is covered with nano-ceramic powder of about 30-50 μm thickness. The drying time after the last dipping is 24 hours.

[0038] (4) After sieving boron carbide (B4C), silicon carbide (SiC), silicon dioxide (SiO2), aluminum oxide (Al2O3) and boron trioxide (B2O3) powders (the particle size of the above five powders is 3-5μm), they are weighed according to 25wt.% boron carbide, 25wt.% silicon carbide, 15wt.% silicon dioxide, 15wt.% aluminum oxide and 20wt.% boron trioxide, and then ball-milled with alcohol at a solid-liquid mass ratio of 1:1 for 10h to obtain micron-sized powder slurry.

[0039] (5) Apply two coats of the micron powder slurry obtained in step (4) with a thickness of about 50 to 100 μm to the surface of the lightweight carbon-based composite material substrate with nanoparticles obtained in step (3) using a brushing process. After air drying, dry at 120°C for 2 hours for later use.

[0040] (6) According to 4g / cm 2 High-purity silicon powder was evenly sprinkled around the bottom of the graphite crucible. The substrate material dried in step (5) was placed on top of the silicon powder and placed in a high-temperature furnace for high-temperature treatment: the temperature was raised from room temperature to the target temperature of 1500℃ at a rate of 10℃ / min. After holding at the target temperature for 2 hours, the sample was cooled to room temperature and removed. Finally, a SiC nanowire-toughened gradient SiC ceramic layer was obtained in situ on the surface of the lightweight carbon-based composite material, thus realizing the preparation of a lightweight carbon-ceramic heat insulation integrated material.

[0041] The surface layer of the lightweight carbon-ceramic integrated heat-insulating material obtained by the above steps is a SiC nanowire-toughened gradient SiC ceramic layer with a thickness of approximately 750 μm (e.g., Figure 1 As shown in Figure a), a large number of nanowires with diameters of approximately 20–50 nm can be observed within a thickness of approximately 150 μm from the surface (e.g., ...). Figure 1 (as shown in b); the bottom layer is an unreacted lightweight carbon-based composite material substrate, still possessing nanoscale (diameter approximately 70–100 nm) properties. Figure 1 c) Porous carbon three-dimensional network framework. The material did not crack or peel after 10 thermal shocks from room temperature to 1700℃, and its microstructure remained as shown. Figure 2 As shown; a 10mm thick material was ablated at 1700℃ for 300s with oxyacetylene, and the ablated surface was smooth (as shown). Figure 3 As shown), the ablation temperature on the back side is only 700℃, exhibiting excellent heat insulation performance (e.g. Figure 4 (As shown).

[0042] Example 2

[0043] (1) With a density of 0.4 g / cm³ 3 Using lightweight carbon-based composite material (C / CA, Institute of Metal Research, Chinese Academy of Sciences) as the substrate, the material was processed into a cylinder with a diameter of 30 mm and a thickness of 10 mm. After ultrasonic cleaning with alcohol, the cylinder was dried in an oven at 100°C for 24 hours before use.

[0044] (2) Weigh out the following nano-ceramic powders according to the following mass ratio: 25 wt.% ZrO2 powder, 50 wt.% C powder, and 25 wt.% Al2O3 powder; mix the above nano-ceramic powders with dispersant (polyethyleneimine, PEI) and deionized water in a mass ratio of 2:1:1 and stir on a magnetic stirrer for 8 hours until the ceramic powders are uniformly dispersed in the deionized water; transfer the above solid-liquid mixture into a ball mill jar and ball mill for 5 hours to obtain a nano-ceramic powder slurry.

[0045] (3) The lightweight carbon-based composite material substrate is completely immersed in the nano-ceramic powder slurry. After dipping in the slurry for 5 seconds, it is taken out and dried at 100°C. The above immersion, dipping and drying operations are repeated twice until the substrate surface is covered with nano-ceramic powder of about 30-50 μm thickness. The drying time after the last dipping is 24 hours.

[0046] (4) After sieving boron carbide (B4C), silicon carbide (SiC), silicon dioxide (SiO2), aluminum oxide (Al2O3) and boron trioxide (B2O3) powders (the particle size of the above five powders is 3-5μm), they are weighed according to 25wt.% boron carbide, 25wt.% silicon carbide, 15wt.% silicon dioxide, 15wt.% aluminum oxide and 20wt.% boron trioxide, and then ball-milled with alcohol at a solid-liquid mass ratio of 1:1 for 10h to obtain micron-sized powder slurry.

[0047] (5) Apply two coats of the micron powder slurry obtained in step (4) with a thickness of about 50 to 100 μm to the surface of the lightweight carbon-based composite material substrate with nanoparticles obtained in step (3) using a brushing process. After air drying, dry at 120°C for 2 hours for later use.

[0048] (6) According to 3g / cm 2High-purity silicon powder was evenly sprinkled around the bottom of the graphite crucible. The substrate material dried in step (5) was placed on top of the silicon powder and placed in a high-temperature furnace for high-temperature treatment: the temperature was raised from room temperature to the target temperature of 1400℃ at a rate of 8℃ / min. After holding at the target temperature for 1 hour, the sample was cooled to room temperature and removed. Finally, a SiC nanowire-toughened gradient SiC ceramic layer was obtained in situ on the surface of the lightweight carbon-based composite material, thus realizing the preparation of a lightweight carbon-ceramic heat insulation integrated material.

[0049] The surface layer of the lightweight carbon-ceramic integrated heat-insulating material obtained by the above steps is a SiC nanowire-toughened gradient SiC ceramic layer with a thickness of approximately 750 μm (e.g., Figure 5 As shown in a), within a thickness of approximately 150 μm from the surface to the outermost layer, a large number of nanowires with diameters of approximately 20–50 nm can be observed (e.g., ...). Figure 5 (as shown in b); the bottom layer is an unreacted lightweight carbon-based composite material substrate, still possessing nanoscale (diameter approximately 70–100 nm) properties. Figure 5 c) Porous carbon three-dimensional network framework. The material did not crack or peel after 10 thermal shocks from room temperature to 1700℃, and its microstructure remained as shown. Figure 6 As shown; after five cycles of oxyacetylene ablation at 1700℃ for 300s, the 10mm thick material had a smooth ablation surface without exposing the substrate (as shown). Figure 7 (As shown). Because the carbon substrate has a lower density than in Example 1, it exhibits better thermal insulation performance, with the ablation temperature on the back side further reduced to 570°C, demonstrating excellent thermal insulation properties (e.g.). Figure 8 (As shown).

[0050] Comparative Example 1

[0051] (1) With a density of 0.6 g / cm³ 3 Using lightweight carbon-based composite material (C / CA, Institute of Metal Research, Chinese Academy of Sciences) as the substrate, the material was processed into a cylinder with a diameter of 30 mm and a thickness of 10 mm. After ultrasonic cleaning with alcohol, the cylinder was dried in an oven at 100°C for 24 hours before use.

[0052] (2) After sieving boron carbide (B4C), silicon carbide (SiC), silicon dioxide (SiO2), aluminum oxide (Al2O3) and boron trioxide (B2O3) powders (the particle size of the above five powders is 3-5μm), they are weighed according to 25wt.% boron carbide, 25wt.% silicon carbide, 15wt.% silicon dioxide, 15wt.% aluminum oxide and 20wt.% boron trioxide, and then ball-milled with alcohol at a solid-liquid mass ratio of 1:1 for 10h to obtain micron-sized powder slurry.

[0053] (3) The micron powder slurry obtained in step (2) is applied in two coats with a thickness of about 50 to 100 μm to the surface of the lightweight carbon-based composite material substrate with nanoparticles obtained in step (3). After natural air drying, it is dried at 120°C for 2 hours for later use.

[0054] (6) According to 3g / cm 2 High-purity silicon powder was evenly sprinkled around the bottom of the graphite crucible. The substrate material dried in step (3) was placed on top of the silicon powder and placed in a high-temperature furnace for high-temperature treatment: the temperature was raised from room temperature to the target temperature of 1400℃ at a rate of 8℃ / min. After holding at the target temperature for 1 hour, the sample was cooled to room temperature and taken out.

[0055] The coating thickness obtained by the above steps is approximately 350 μm (e.g. Figure 9 As shown in a), no nanowires were observed within a thickness of approximately 100 μm from the surface to the surface layer (as shown in a). Figure 9 (As shown in b). This is because the growth of nanowires requires the reaction intermediate CO, but the comparative example lacks nanoscale oxides such as SiO2, ZrO2, or Al2O3 to react with C to generate CO, making it difficult for nanowires to nucleate and grow. Therefore, in Example 1, the nanowire induction layer significantly promotes nanowire formation.

Claims

1. A method for preparing a lightweight carbon-ceramic integrated heat-insulating material with a SiC ceramic layer, characterized in that: This method employs a low-temperature gas-solid reaction ceramicization technique induced by nanopowder to SiC nanowires, achieving the preparation of a lightweight carbon-ceramic integrated heat-insulating material with a SiC nanowire-toughened gradient SiC ceramic layer. The specific steps include: (1) lightweight carbon-based composite material with density 0.2-0.8 g / cm 3 as a substrate; (2) Weigh nano-ceramic powder, dispersant PEI and water into a container and stir until the ceramic powder is dispersed in water to obtain a solid-liquid mixture; transfer the above solid-liquid mixture into a ball mill jar and ball mill for 3-5 hours to obtain nano-ceramic powder slurry; The nano-ceramic powder slurry contains any one of the following three components: Nano-ceramic powder 1: ZrO2 powder 10-20 wt.%, C powder 30-50 wt.%, SiO2 powder 30-50 wt.%; Nano-ceramic powder 2: ZrO2 powder 10-30 wt.%, C powder 40-60 wt.%, Al2O3 powder 20-50 wt.%; Nano-ceramic powder 3: Al2O3 powder 20-30 wt.%, C powder 30-40 wt.%, SiO2 powder 40-50 wt.%; (3) Immerse the lightweight carbon-based composite material substrate completely in the nano-ceramic powder slurry, take it out after 3-5 seconds of dipping in the slurry, dry the surface at 80-120ºC, and repeat the above dipping and drying operation 0-4 times until the substrate surface is covered with 30-50μm thick nano-ceramic powder. (4) After sieving the boron carbide, silicon carbide, silicon dioxide, aluminum oxide and boron trioxide powders, weigh them according to the following proportions: boron carbide 20~25wt.%, silicon carbide 20~25wt.%, silicon dioxide 15~20wt.%, aluminum oxide 10~15wt.%, boron trioxide 20~25wt.%, and then ball-mill them with alcohol for 8~10h to obtain micron-sized powder slurry; the particle size of the above five powders is 3~5μm; (5) Apply the micron powder material obtained in step (4) twice to the surface of the lightweight carbon-based composite material substrate with nanoparticles obtained in step (3) using a brushing process. The thickness is 50-100μm. After air drying, dry it at 100-130ºC for 2-5 hours for later use. (6) Sprinkle silicon powder evenly on the bottom of the graphite crucible, place the substrate material dried in step (5) on top of the silicon powder, and place it in a high-temperature furnace for high-temperature treatment: heat from room temperature to the target temperature of 1300~1600ºC at a heating rate of 5-10ºC / min, keep at the target temperature for 1-5 hours, cool to room temperature and take out the sample. Finally, a SiC nanowire toughened gradient SiC ceramic layer is obtained in situ on the surface of the lightweight carbon-based composite material, realizing the preparation of lightweight carbon-ceramic heat insulation integrated material.

2. The preparation method according to claim 1, characterized in that: In step (2), the content of powder in the nano-ceramic powder slurry is 40~50wt.%, the content of dispersant PEI is 20~30wt.%, and the remainder is water.

3. The preparation method according to claim 1, characterized in that: In step (2), the nano-ceramic powder, dispersant PEI, and water are weighed into a container and stirred for 5-10 hours until the ceramic powder is dispersed in deionized water. The solid-liquid mixture is then transferred into a ball mill jar and ball-milled for 3-5 hours to obtain a nano-ceramic powder slurry.

4. The preparation method according to claim 1, characterized in that: In step (3), the lightweight carbon-based composite material substrate is dipped in slurry 1-5 times; the drying time after the last dip is 24-48 hours.

5. The preparation method according to claim 1, characterized in that: In step (4), the powder and alcohol are mixed at a solid-liquid mass ratio of 1:1 to 1.

5.

6. The preparation method according to claim 1, characterized in that: In step (6), the amount of high-purity silicon powder sprinkled in the graphite crucible is 1-8 g / cm2, the purity of the silicon powder is 99%, and the particle size is 1-3 μm.

7. The preparation method according to claim 1, characterized in that: In step (1), a lightweight carbon-based composite material with a density of 0.2~0.8 g / cm3 is used as the base, processed into the required shape, ultrasonically cleaned with alcohol, and then dried in an oven at 80-120ºC for 24-48 hours for later use.

8. A lightweight carbon-ceramic integrated heat-insulating material prepared by any one of claims 1 to 7, characterized in that: The material consists of a 100-600 μm thick SiC nanowire-toughened gradient SiC ceramic layer on the surface and an unreacted lightweight carbon-based composite substrate at the bottom. The material did not crack or peel after 10 thermal shocks at room temperature to 1700 ºC. After 5 cycles of oxyacetylene ablation at 1700ºC for 300 s, the surface remained smooth, and the back temperature of a 10 mm sample was 700ºC, demonstrating excellent heat insulation performance.

Citation Information

Patent Citations

  • Heat protection, heat insulation and bearing integrated light carbon-ceramic composite material and preparation method thereof