A polyester blended yarn and its production process

By modifying polyester fibers with branched polyols and composite dicarboxylic acids through condensation and three-dimensional network graphene, the porosity is increased and the fiber surface is roughened, thus solving the problem of poor breathability of polyester fiber fabrics and achieving good breathability and antistatic effects.

CN119145096BActive Publication Date: 2026-11-17YIBIN TIANZHIHUA TEXTILE TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411294140.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2026-11-17
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

Existing polyester fiber fabrics have poor breathability after antistatic treatment, which affects user comfort.

Method used

Polymerization of branched polyols and complex dicarboxylic acids is carried out, combined with three-dimensional network graphene modification, to form polyester fibers with high steric hindrance, which increases pore size and makes the fiber surface rough and fluffy, promotes air flow and reduces static electricity accumulation.

Benefits of technology

It improves the breathability and antistatic properties of polyester fibers, while maintaining good user comfort and antistatic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045435350000161
    Figure BDA0005045435350000161
  • Figure BDA0005045435350000171
    Figure BDA0005045435350000171
Patent Text Reader

Abstract

This invention relates to the field of polyester fabric technology. Addressing the issue that existing antistatic polyester fiber fabrics often achieve their antistatic effect by adding or covering antistatic materials, which further exacerbates the poor breathability of polyester fabrics, this invention discloses a polyester blended yarn and its production process. The production process of the polyester blended yarn includes the following steps: S1, mixing a composite diacid with a polyol, adding three-dimensional network graphene, mixing thoroughly, and heating in an inert gas atmosphere; then adding a polycondensation catalyst and continuing the reaction to obtain a polyester melt, which is then extruded and spun to obtain polyester fibers; S2, mixing the polyester fibers obtained in step S1 with collagen fibers, impregnating in a carbonate solution, ultrasonically dispersing, heating and drying, and then weaving in a twill weave to obtain the polyester blended yarn. By improving the polyester fiber polycondensation raw material and combining it with three-dimensional network graphene, a good balance of antistatic effect and breathability is achieved simultaneously.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyester fabric technology, and more specifically, to a polyester blended yarn and its production process. Background Technology

[0002] Polyester fiber is a synthetic fiber made from organic diacids and diols through a chemical polycondensation reaction, commonly known as polyester. Polyester has excellent wrinkle resistance and shape retention, making clothing made from it less prone to wrinkling during wear and able to maintain its original shape. It also has high strength and elastic recovery ability, making the woven fabrics strong and durable, and able to quickly return to their original shape. In addition, it is also abrasion resistant and does not attract lint, making the fabric look neater.

[0003] However, polyester fibers generate static electricity during production and use, attracting a large amount of dust and affecting the production environment and user comfort. To address this, patent CN115723400A provides an antistatic warp-knitted fabric and its preparation process. It uses modified polyester and wool fibers as skin-friendly raw materials, and sequentially sets up an insulation layer, an antistatic layer, and an antibacterial layer. The modified polyester fibers have good hydrophobicity, tensile strength, and antistatic ability, effectively improving the waterproof effect, tensile strength, and antistatic effect of the textile fabric, thereby effectively improving the performance of the textile fabric.

[0004] In addition to antistatic properties, existing polyester fiber fabrics also face performance requirements such as warmth and breathability. However, existing antistatic polyester fiber fabrics mostly achieve their antistatic effect by adding or covering them with antistatic materials, which further aggravates the problem of poor breathability of polyester fabrics. Summary of the Invention

[0005] The technical problem to be solved by this invention:

[0006] Currently, to address the problem of static electricity in polyester fiber fabrics, the main approach is to modify the polyester fibers by adding or covering them with anti-static materials. However, while these methods can solve the problem of severe static electricity in polyester fiber fabrics, they also make the already poorly breathable polyester fiber fabrics even less breathable and less absorbent, thus affecting their comfort during use.

[0007] The technical solution adopted in this invention is as follows:

[0008] This invention provides a production process for polyester blended yarn, comprising the following steps:

[0009] S1 mixes a composite dicarboxylic acid with a polyol, adds a three-dimensional network graphene, mixes well, places it in an inert gas atmosphere, and heats it to react; then a polycondensation catalyst is added, and the temperature is raised to continue the reaction to obtain a polyester melt, which is then extruded and spun to obtain polyester fiber.

[0010] S2 mixes the polyester fiber obtained in step S1 with collagen fiber, immerses it in a carbonic acid solution, ultrasonically disperses it, heats and dries it, and then weaves it in a twill pattern to obtain the polyester blended yarn.

[0011] Preferably, in step S1, the method for preparing the three-dimensional network graphene includes the following steps:

[0012] Carbon nanomaterials were placed in an inert gas environment and heated to above 1450°C, then allowed to stand. The material was then transferred to a methane solution, stirred and soaked, cooled to below 1000°C, allowed to stand and react, and then cooled to room temperature to obtain the three-dimensional network graphene.

[0013] Preferably, the heating rate of the carbon nanomaterial in an inert gas environment is 8-25℃ / s.

[0014] Preferably, the particle size of the carbon nanomaterial is 500-800 nm.

[0015] Preferably, in step S1, the pressure of the inert gas atmosphere is less than 0.5 MPa.

[0016] Preferably, in step S1, the initial heating temperature is 135-155℃, and the reaction time is 1.5-3.2 hours.

[0017] The heating temperature after adding the polycondensation catalyst is 220-250℃, and the reaction time is 0.75-1.2h.

[0018] Preferably, the complex dicarboxylic acid includes an organic dicarboxylic acid and maleic anhydride, wherein the organic dicarboxylic acid can be selected from one or more of 1,4-succinic acid, 1,6-adipic acid, octanoic acid, and azelaic acid; and the polyol molecule contains a branched structure.

[0019] Preferably, the polyol may be selected from one or more of 1,6-hexanediol and 2-butyl-2-ethyl-1,3-propanediol.

[0020] Preferably, in step S2, the mass ratio of polyester fiber to collagen fiber is 1-1.2:0.85-1.05.

[0021] The beneficial effects of this invention are as follows:

[0022] In the production process of the polyester blended yarn of the present invention, polyols with branched structures and complex dicarboxylic acids are polycondensed to form polyester fibers with relatively higher steric hindrance. This increases the spatial porosity of the polyester fibers, making the air circulation path more diverse, thereby improving the air permeability of the polyester fibers. Moreover, within a certain range, the relatively higher steric hindrance can reduce the contact area between polyester fibers, thereby reducing the accumulation of static electricity and achieving the effect of reducing static electricity generation.

[0023] Furthermore, the introduction of three-dimensional network graphene with a spatial three-dimensional structure into the polyester fiber gives it a rough, plush surface, promoting airflow on its surface and thus improving the breathability of the polyester fiber yarn. The roughness of its surface can also alleviate electron transfer caused by friction, thereby reducing the formation of static charge and exerting an antistatic effect, thus achieving both good antistatic effect and breathability. Detailed Implementation

[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0025] This invention provides a polyester blended yarn and its manufacturing process, the manufacturing process comprising the following steps:

[0026] (1) Preparation of polyester fibers

[0027] A composite dicarboxylic acid and a polyol are mixed in stoichiometric ratio, and three-dimensional network graphene is added. The mixture is stirred and homogenized, placed in a closed reactor, and an inert gas is introduced until the pressure inside the reactor is less than 0.5 MPa. The mixture is then heated to 135-155℃ and stirred for 1.5-3.2 h. A polycondensation catalyst is then added, and the mixture is heated to 220-250℃ and reacted for 0.75-1.2 h to obtain a polyester melt. Finally, polyester fibers are prepared by extrusion spinning.

[0028] Among them, the complex dicarboxylic acid includes organic dicarboxylic acid and maleic anhydride. The organic dicarboxylic acid can be selected from one or more of 1,4-succinic acid, 1,6-adipic acid, octanoic acid, azelaic acid, etc.; the polyol molecule contains a branched structure and can be selected from one or more of 1,6-hexanediol and 2-butyl-2-ethyl-1,3-propanediol, etc.

[0029] (2) Preparation of polyester blended yarn

[0030] The polyester fiber prepared above is mixed with collagen fiber at a mass ratio of 1-1.2:0.85-1.05, immersed in a carbonic acid solution, ultrasonically dispersed for 30-45 minutes, heated and dried, and then twill woven to obtain polyester blended yarn.

[0031] In this invention, the preparation method for three-dimensional network graphene in polyester fibers includes the following steps:

[0032] Carbon nanomaterials are placed in an inert gas environment and rapidly heated to above 1450℃ at 8-25℃ / s, then allowed to stand for 3-5 minutes. They are then transferred to a methane solution, soaked and stirred for 3-10 minutes until the temperature drops below 1000℃, and allowed to stand for 2-3.5 hours. After cooling to room temperature, three-dimensional network graphene is obtained, which has a spatial three-dimensional network structure, good bonding strength, and can enrich the surface spatial structure of polyester fibers, making its surface appear as a porous, fluffy texture.

[0033] Among them, carbon nanomaterials can be any one or more of carbon nanotubes, carbon nanofibers, and nanographite powder, and the particle size of carbon nanomaterials is 500-800nm.

[0034] This invention modifies polyester fibers to give them a rough, plush surface, promoting airflow and thus improving the breathability of the polyester yarn. The rough surface also reduces electron transfer caused by friction, thereby reducing static charge formation and providing antistatic properties. This allows for the simultaneous achievement of both good antistatic effects and breathability.

[0035] Example 1

[0036] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0037] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 h; then add 0.3 wt% triethanolamine, and further heat to 240°C and react for 1 h to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0038] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0039] Example 2

[0040] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 530±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0041] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0042] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0043] Example 3

[0044] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 750±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0045] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0046] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0047] Example 4

[0048] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0049] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 12 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0050] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0051] Example 5

[0052] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0053] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 35 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0054] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0055] Example 6

[0056] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0057] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 80 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0058] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0059] Example 7

[0060] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0061] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 130 parts by mass of 1,6-hexanediol, and add three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0062] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0063] Example 8

[0064] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0065] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 136°C and stir for 3.2 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0066] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0067] Example 9

[0068] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0069] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 155°C and stir the reaction for 1.65 h; then add triethanolamine, and further heat to 240°C and react for 1 h to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0070] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0071] Example 10

[0072] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0073] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 h; then add triethanolamine, and further heat to 225°C and react for 1.2 h to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0074] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0075] Example 11

[0076] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0077] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 h; then add triethanolamine, and further heat to 250°C and react for 0.75 h to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0078] Step 3: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0079] Example 12

[0080] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0081] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0082] Step 3: Take 12 parts by weight of polyester fiber and 8.6 parts by weight of collagen fiber, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0083] Example 13

[0084] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0085] Step 2: Take 70 parts by mass of 1,4-succinic acid, 39.2 parts by mass of maleic anhydride, and 118 parts by mass of 1,6-hexanediol, and add 25 parts by mass of three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0086] Step 3: Take 10.5 parts by weight of polyester fiber and 11 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester blended yarn by twill weaving.

[0087] Comparative Example 1

[0088] Step 1: Take 1,4-succinic acid, maleic anhydride and 1,6-hexanediol, stir and mix them, place them in a closed reactor, introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir the reaction for 2.5 h; then add triethanolamine, further heat to 240°C, and react for 1 h to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0089] Step 2: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester yarn by twill weaving.

[0090] Comparative Example 2

[0091] Step 1: Take terephthalic acid and ethylene glycol, stir and mix them, place them in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor, and control the internal pressure of the reactor to about 0.3 MPa; then heat the reactor to 150°C and stir the reaction for 2.5 hours; then add triethanolamine, and further heat to 240°C and react for 1 hour to obtain polyester melt, which is then extruded and spun to obtain polyester fiber.

[0092] Step 2: Take 15.5 parts by weight of polyester fiber and 13.8 parts by weight of collagen fiber respectively, mix them, soak them in a carbonic acid solution for 2 hours, and then ultrasonically disperse them for 40 minutes. After that, heat them to about 85°C and dry them. Then, prepare polyester yarn by twill weaving.

[0093] Comparative Example 3

[0094] Step 1: Take 20 parts by mass of carbon nanotubes with a particle size of 600±20nm, place them in a high-temperature furnace, introduce argon gas and exhaust the air, heat at a heating rate of 10℃ / s to about 1500℃, keep at this temperature and let stand for 3.5min; take out the carbon nanotubes and place them in twice the volume of methane solution, stir at 550rpm for 5min until the temperature drops below 1000℃, keep at this temperature and let stand for 2.5h, take out the carbon nanotubes and cool to room temperature to obtain three-dimensional network graphene.

[0095] Step 2: Take 1,4-succinic acid, maleic anhydride, and 1,6-hexanediol, and add three-dimensional network graphene. Stir and mix well, place in a sealed reactor, and introduce equal volumes of argon and hydrogen to fully fill the internal environment of the reactor. Control the internal pressure of the reactor to about 0.3 MPa. Then heat the reactor to 150°C and stir for 2.5 hours. Add triethanolamine and further heat to 240°C and react for 1 hour to obtain polyester melt. After extrusion spinning, obtain polyester fiber.

[0096] Step 3: Take polyester fiber, soak it in a carbonic acid solution for 2 hours, and then ultrasonically disperse it for 40 minutes. After drying, heat it to about 85°C and then weave it in a twill pattern to obtain polyester yarn.

[0097] Test case

[0098] Samples: Examples 1-13, Comparative Examples 1-3

[0099] Polyester yarns prepared in Examples 1-13 and Comparative Examples 1-3 were taken as samples, and the material properties such as moisture permeability of each sample were measured in turn. The measurement methods and test results are summarized in Table 1 below:

[0100] Table 1. Material property test results of different samples

[0101]

[0102]

[0103] As shown in Table 1 above, the polyester yarns prepared in Examples 1 to 13 exhibit significantly better performance than the polyester yarns prepared in Comparative Examples 1 to 3 in terms of moisture permeability, air permeability, and resistivity. Therefore, it can be demonstrated that the polyester blended yarn and its production process used in this invention can improve upon the shortcomings of existing polyester blended yarns, such as poor air permeability and lack of moisture absorption, while maintaining good antistatic properties.

[0104] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A production process for polyester blended yarn, characterized in that, Includes the following steps: S1 involves mixing a composite dicarboxylic acid with a polyol, adding a three-dimensional network of graphene, mixing thoroughly, and placing the mixture in an inert gas atmosphere with a pressure less than 0.5 MPa for heating and reaction. Then, a polycondensation catalyst is added, and the temperature is raised further to obtain a polyester melt, which is then extruded and spun to obtain polyester fibers. The complex dicarboxylic acid includes an organic dicarboxylic acid and maleic anhydride. The organic dicarboxylic acid is selected from one or more of 1,4-succinic acid, 1,6-adipic acid, octanoic acid, and azelaic acid; and the polyol molecule contains a branched structure. The method for preparing the three-dimensional network graphene includes the following steps: Carbon nanomaterials were placed in an inert gas environment and heated to above 1450°C, then allowed to stand. The mixture was then transferred to a methane solution, stirred and soaked, cooled to below 1000°C, allowed to stand and react, and then cooled to room temperature to obtain the three-dimensional network graphene. S2. The polyester fiber obtained in step S1 is mixed with collagen fiber at a mass ratio of 1-1.2:0.85-1.

05. The mixture is then immersed in a carbonic acid solution, ultrasonically dispersed, and heated and dried to obtain the polyester blended yarn.

2. The production process of polyester blended yarn according to claim 1, characterized in that, The heating rate of carbon nanomaterials in an inert gas environment is 8-25℃ / s.

3. The production process of polyester blended yarn according to claim 1, characterized in that, The particle size of carbon nanomaterials is 500-800 nm.

4. The production process of polyester blended yarn according to claim 1, characterized in that, In step S1, the initial heating temperature is 135-155℃, and the reaction time is 1.5-3.2h; The heating temperature after adding the polycondensation catalyst is 220-250℃, and the reaction time is 0.75-1.2h.

5. The production process of polyester blended yarn according to claim 1, characterized in that, The polyol is selected from one or more of 1,6-hexanediol and 2-butyl-2-ethyl-1,3-propanediol.

6. Polyester blended yarn prepared using the production process described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Anti-static warp-knitted fabric and preparation process thereof

    CN115723400A

  • Graphene-containing composite polyester fiber and its preparation method and use

    CN105525381A

  • Graphene / carbon nanotube network flexible multifunctional strain sensor preparation method

    CN106767374A

  • Preparation method of carbon fiber / carbon nano tube / organic silicon modified unsaturated polyester nano composite material

    CN115160797A

  • Humectant cloth and undergarment including same

    WO2022230609A1