A method for combined treatment of secondary aluminum ash by wet washing and high-temperature calcination
By employing a combined wet washing and high-temperature calcination method, and utilizing ammonium chloride solution for washing and optimizing process parameters, the high energy consumption and pollution problems in secondary aluminum ash treatment were solved, achieving efficient resource utilization and the preparation of high-alumina refractory materials.
Patent Information
- Application Number
- CN202411368731.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-09-29
AI Technical Summary
Existing secondary aluminum ash treatment technologies suffer from high energy consumption, large acid and alkali consumption, heavy pollution, severe equipment corrosion, and low resource utilization. Furthermore, both wet and pyrometallurgical treatments have their drawbacks, and there is a lack of economical and efficient treatment processes.
A combined wet washing and high-temperature calcination method was adopted. First, soluble salts and alkali metal elements were removed by washing with ammonium chloride solution. Then, high-temperature calcination was carried out to optimize process parameters to increase alumina content and prepare high-alumina refractory materials.
It effectively removes harmful impurities from secondary aluminum ash, increases alumina content, meets the quality requirements of refractory materials, realizes high-value utilization of resources, and reduces operating costs and environmental pollution.
Smart Images

Figure BDA0005066988580000041 
Figure HDA0005066988590000011 
Figure HDA0005066988590000012
Abstract
Description
Technical Field
[0001] This invention belongs to the field of secondary aluminum ash resource utilization technology, specifically relating to a method for combined treatment of secondary aluminum ash by wet washing and high-temperature roasting. Background Technology
[0002] In the electrolytic aluminum, aluminum processing, and recycled aluminum industries, the dross generated during the smelting and casting of aluminum or aluminum alloys is called primary aluminum ash. The slag produced after melting and extracting aluminum from primary aluminum ash is secondary aluminum ash, which has a very complex composition, mainly including alumina, magnesium aluminum spinel, aluminum nitride, metallic aluminum, chlorides, and fluorides, possessing both resource-related and polluting properties. Secondary aluminum ash has been included in the 2021 edition of the "National Hazardous Waste List" and is classified as hazardous solid waste. Due to the lack of low-cost, large-scale, and relatively mature treatment processes, aluminum production enterprises currently mainly dispose of secondary aluminum ash through traditional stockpiling or landfill methods. This not only fails to effectively utilize valuable metallic aluminum but also leads to problems such as occupying land resources and causing environmental pollution. Therefore, exploring an economical, environmentally friendly, and efficient disposal method is key to the resource utilization of secondary aluminum ash.
[0003] Extensive research and practice have been conducted to address this challenge. Chinese patent document (application number: CN202410309546.9) discloses a method for efficiently and harmlessly treating secondary aluminum ash. This method involves mixing ground and sieved secondary aluminum ash with a sodium hydroxide solution for hydrolysis and denitrification. After denitrification, a mixture of lime and calcium chloride is added to remove fluoride, effectively removing nitrogen and fluoride ions from the secondary aluminum ash. However, this process does not consider changes in the content of valuable aluminum. Chinese patent document (application number: CN202310832015.3) discloses a combined treatment method for secondary aluminum ash: ball milling and sorting, low-temperature roasting, and water washing and leaching. This method involves particle size sorting of the secondary aluminum ash, low-temperature roasting of medium-sized particles, and low-temperature roasting of fine-sized particles using doped aluminum electrolyte. After treatment, the medium, fine, and coarse-sized particles are all subjected to water washing and leaching to obtain harmless secondary aluminum ash and inorganic salts. This method achieves effective recovery of inorganic salts, but the direct roasting process easily causes flue gas corrosion of equipment and pipelines, reducing their service life. Chinese patent document (application number: CN202311783106.9) discloses a method for the resource utilization of secondary aluminum ash, employing ultrasonic-enhanced alkaline leaching. The leaching solution is then processed through seed crystal separation, roasting, and dehydration to produce high-grade alumina raw materials, and the leaching residue is used to prepare high-performance adsorbent materials. Although this method has a short process flow, it still suffers from problems such as high cost of alkaline additives, large dosage requirements, and long reaction times. Chinese patent document (application number: CN202310348500.3) discloses a method for the resource treatment of secondary aluminum ash, obtaining a polyaluminum chloride solution through alkaline leaching, acid leaching, roasting activation, and leaching processes, achieving the recovery and recycling of aluminum from the secondary aluminum ash. However, this method suffers from drawbacks such as high acid and alkali consumption and low aluminum ash residue recovery rate.
[0004] In the process of utilizing secondary aluminum ash resources, two main technical routes have been established for its treatment and disposal: wet processing and pyrometallurgical processing. Wet processing mainly involves acid washing and alkali washing. Research has found that while wet processing has low energy consumption, it suffers from drawbacks such as complex process conditions, high acid and alkali consumption, and severe secondary pollution. Pyrometallurgical processing, namely high-temperature roasting, not only imposes strict limits on the impurity content in the secondary aluminum ash but also generates large volumes of complex flue gas and causes pipeline corrosion. Currently, there are few industrial-scale cases of secondary aluminum ash treatment; most are still in the laboratory research stage. In practical applications, specific process routes need to be customized for different utilization methods. Summary of the Invention
[0005] In view of the shortcomings and deficiencies of existing technologies for the resource utilization of secondary aluminum ash, this invention proposes for the first time a combined treatment method of wet washing and high-temperature roasting by comparing the advantages and disadvantages of wet and pyrometallurgical processes for secondary aluminum ash.
[0006] First, the secondary alumina ash undergoes wet washing to remove most of the soluble salts and alkali metal elements, reducing flue gas emissions during calcination and preventing the impact of alkali metal elements on the performance of high-alumina refractories. Second, the secondary alumina ash is then subjected to high-temperature calcination to increase the alumina content, ensuring the quality and stability of the material. Simultaneously, the process parameters for wet washing and high-temperature calcination of the secondary alumina ash are designed and optimized to reduce operating costs and improve processing efficiency. Furthermore, for the first time, ammonium chloride solution is used as the washing liquid in the wet washing process, effectively increasing the alumina content while maintaining the removal rate of alkali metal elements, thus enhancing the quality of high-alumina refractories.
[0007] The technical solution of the present invention is as follows:
[0008] A method for combined treatment of secondary aluminum ash by wet washing and high-temperature calcination includes the following steps:
[0009] (1) Preprocessing
[0010] Secondary aluminum ash is obtained by sieving and dry ball milling to obtain secondary aluminum ash with uniform particle size.
[0011] Secondary aluminum ash includes secondary aluminum ash generated from any of the industries such as aluminum electrolysis, aluminum recycling, or aluminum processing.
[0012] Specifically, sieving refers to: passing the secondary aluminum ash through a 60-mesh standard sieve, with a cumulative yield of oversize material greater than 98%; the oversize material is then subjected to dry ball milling to obtain secondary aluminum ash with uniform particle size; the ball mill speed for dry ball milling is controlled at 200-400 r / min (preferably 300 r / min), and the time is controlled at 10-60 min (preferably 30 min);
[0013] (2) Wet washing
[0014] The secondary aluminum ash obtained in step (1) is mixed with a water washing solution and washed to obtain a secondary aluminum ash water washing sample.
[0015] The washing solution is ultrapure water or an aqueous solution of ammonium chloride; preferably, the aqueous solution of ammonium chloride has a mass fraction of 5-20%, for example, 5%, 10%, 15%, 20%, and particularly preferably 15%;
[0016] The preferred solid-liquid ratio of secondary aluminum ash to washing solution is 1:1 to 5, g / mL; for example, 1:1, 1:2, 1:3, 1:4, 1:5, g / mL; the optimal solid-liquid ratio is 1:3, g / mL.
[0017] The preferred washing temperature is 10–100℃, for example, 20, 40, 60, 80, or 100℃; the optimal washing temperature is 60℃.
[0018] The preferred washing time is 1 to 5 hours, for example, 1, 2, 3, 4, or 5 hours; the optimal washing time is 3 hours.
[0019] The preferred water washing stirring speed is 100-1000 r / min, for example, 200, 400, 600, 800, 1000 r / min; the optimal water washing stirring speed is 600 r / min.
[0020] (3) High-temperature roasting
[0021] The secondary aluminum ash water-washed sample obtained in step (3) was subjected to high-temperature calcination to obtain high-alumina refractory material;
[0022] The high-temperature roasting temperature is 700–1500℃, for example, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500℃; the roasting time is 1–5 hours, for example, 1, 2, 3, 4, 5 hours.
[0023] The optimal calcination temperature is 1300℃, and the optimal calcination time is 4h.
[0024] The preferred heating rate for high-temperature calcination is 6℃ / min;
[0025] The roasting atmosphere is air, and the gas flow rate is 4 L / min.
[0026] This invention proposes for the first time a combined wet washing and high-temperature calcination method for treating secondary aluminum ash. It also designs and optimizes the process parameters for both wet washing and high-temperature calcination of secondary aluminum ash, facilitating reduced operating costs and improved processing efficiency. In the wet washing process, ammonium chloride solution is used as the washing liquid for the first time, effectively increasing the alumina content and enhancing the quality of high-alumina refractory materials while maintaining the removal rate of alkali metal elements.
[0027] The technical principles of this invention include:
[0028] There are existing reports on using ammonium chloride as a heavy metal removal agent for the resource utilization of secondary aluminum ash (e.g., CN110548753A). The principle is that ammonium chloride is added to the calcination process of secondary aluminum ash, so that the heavy metal elements contained in the secondary aluminum ash are converted into low-melting-point gaseous compounds, which are then separated from the secondary aluminum ash.
[0029] Unlike previously reported methods, ammonium chloride in this application is used in the wet processing of secondary aluminum ash. Its function is not to remove impurities, but rather to inhibit the hydrolysis of aluminum nitride in the secondary aluminum ash during the washing process, thus stabilizing the alumina content in the washing product. A major problem during the secondary aluminum ash washing process is that AlN reacts with water to form NH3. NH3 is readily soluble in water, which increases the pH of the washing solution, leading to the reaction of AlN, Al(OH)3, and OH... - The reaction produces AlO2 -This leads to a decrease in the alumina content of the washed products; at the same time, the emission of NH3 causes serious environmental problems. NH4Cl is a strong electrolyte that ionizes into NH4 upon dissolving in water. + On the one hand, NH4 + Increased concentration reduces the solubility of NH3 in water, thus hindering the hydrolysis of AlN; on the other hand, NH4 + Hydrolysis binds OH in the solution - H is generated at the same time + It will lower the pH value of the washing solution, thereby inhibiting OH. - It reacts with AlN and Al(OH)3 to form AlO2. - This process reduces the loss of aluminum in the washing products; furthermore, NH4Cl does not react with metallic aluminum, aluminum nitride, aluminum oxide, or other substances.
[0030] This invention uses ammonium chloride solution as the secondary aluminum ash washing solution. Studies have shown that, while ensuring the removal rates of alkali metals K and Na, ammonium chloride solution can effectively inhibit the hydrolysis of aluminum nitride, significantly reduce aluminum loss during the washing process, and stabilize the alumina content in the washing product. This technical feature has not been previously seen in related research or reports.
[0031] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in:
[0032] 1. This invention introduces a combined wet washing and high-temperature roasting process. The wet washing process removes a large amount of soluble salts, such as chlorides and fluorides, from the secondary aluminum ash, preventing these substances from volatilizing into the flue gas during the subsequent high-temperature roasting process, which would lead to complex flue gas composition, difficult separation and recovery, and severe flue corrosion. It also removes alkali metal elements such as potassium and sodium, preventing them from reacting with alumina, silicon dioxide, and other substances to form low-melting-point compounds that would soften the refractory materials. Therefore, wet washing of secondary aluminum ash is particularly crucial.
[0033] 2. This invention optimizes process parameters such as water washing temperature, water washing time, solid-liquid ratio, water washing speed, calcination temperature, and calcination time to obtain optimal process parameters, providing important reference and scientific basis for the harmless treatment and resource utilization of secondary aluminum ash.
[0034] 3. This invention innovatively proposes using ammonium chloride solution as the washing solution, which effectively inhibits aluminum nitride hydrolysis and effectively increases the alumina content while maintaining the removal rate of K and Na.
[0035] 4. By subjecting the optimal water-washed sample of secondary aluminum ash to high-temperature calcination, elements such as N, Cl, F, K, and Na are further removed, while aluminum, aluminum nitride, aluminum carbide, and aluminum hydroxide produced after water washing in the secondary aluminum ash are transformed into stable aluminum oxide.
[0036] 5. After processing, secondary aluminum ash yields a high-alumina refractory material with alumina and magnesium aluminum spinel as the main components. The alumina content reaches approximately 88%, meeting the alumina content (≥80%) requirement in the LZ-80 physicochemical index of GB / T 2988-2012. It can be used directly as aggregate for refractory materials, realizing the high-value resource utilization of secondary aluminum ash. Attached Figure Description
[0037] Figure 1 : A schematic diagram of the process flow of this invention.
[0038] Figure 2 Comparison of physical samples before and after secondary aluminum ash treatment according to the present invention, wherein the left side is the raw material, the middle side is the water-washed sample, and the right side is the calcined sample.
[0039] Figure 3 (a) XRD patterns of secondary aluminum ash before and after water washing; (b) XRD patterns of the optimal water-washed sample and secondary aluminum ash after calcination at 700–1000℃ for 2 hours; (c) XRD pattern of secondary aluminum ash after calcination at 1000–1500℃ for 2 hours; (d) XRD pattern of secondary aluminum ash after calcination at 1300℃ for 1–5 hours.
[0040] Figure 4 The effect of optimal wet washing process parameters on K and Na removal rates (a) and alumina content in Example 2 (b).
[0041] Figure 5 The concentrations of F and Cl ions in the secondary aluminum ash leachate in Example 2 (a) and the mass concentrations of F and Cl ions in the secondary aluminum ash (b).
[0042] Figure 6 Example 3: The main element content (a) and removal rate (b) of secondary aluminum ash washed with ammonium chloride water of different concentrations, and the effect of alumina content (c).
[0043] Figure 7 The effect of different calcination temperatures on the removal rates of K and Na (a) and the alumina content in Example 4 (b).
[0044] Figure 8 The effect of different calcination times on K and Na removal rates (a) and alumina content in Example 4 (b). Detailed Implementation
[0045] The present invention is further described below through specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0046] Taking the secondary aluminum ash produced by a recycling company in my country as an example, the main metallic elements of the secondary aluminum ash raw material processed in this embodiment of the invention, as well as the content of non-metallic elements that need to be paid attention to during the experiment, are shown in Table 1. In addition, the non-metallic elements also include: O (22.6%), N (4.88%), and other trace metallic elements: Mn, Zn, Ni, Ba, etc., which account for about 1%.
[0047] Table 1. Main element content (%) of secondary aluminum ash in Example 1
[0048]
[0049] Pretreatment of secondary aluminum ash
[0050] Screening: Pass the secondary aluminum ash raw material through a 60-mesh standard sieve and mechanically vibrate it to remove large aluminum particles, iron filings, and mixed flocculent matter.
[0051] Ball milling: The secondary aluminum ash undersize material was dry-milled using a drum ball mill for 0.5 hours, with the ball mill speed set to 300 r / min.
[0052] Example 1: Optimization of wet washing process parameters for secondary aluminum ash
[0053] (1) Effect of washing temperature on element removal rate and alumina content
[0054] The pretreated secondary aluminum ash was mixed with a washing solution (ultrapure water). The preferred washing time was 3 hours, the preferred washing speed was 600 r / min, and the preferred solid-liquid ratio was 1:3 g / mL. At a washing temperature of 20℃, the removal rates of K and Na were 43.0% and 53.4%, respectively, and the alumina content was 73%. At a washing temperature of 60℃, the removal rates of K and Na were 50.3% and 70.4%, respectively, and the alumina content was 71.5%. At a washing temperature of 100℃, the removal rates of K and Na were 54.3% and 73.5%, respectively, and the alumina content was 67.1%.
[0055] (2) Effect of washing time on element removal rate and alumina content
[0056] The preferred washing temperature is 60℃, the preferred solid-liquid ratio is 1:3 g / mL, and the preferred washing speed is 600 r / min. With a washing time of 1 h, the removal rates of K and Na are 42.4% and 52.0%, respectively, and the alumina content is 74.8%. With a washing time of 3 h, the removal rates of K and Na are 50.5% and 70.1%, respectively, and the alumina content is 71.6%. With a washing time of 5 h, the removal rates of K and Na are 53.1% and 73.3%, respectively, and the alumina content is 66.6%.
[0057] (3) Effect of solid-liquid ratio on element removal rate and alumina content
[0058] The preferred washing time is 3 hours, the preferred washing temperature is 60℃, and the preferred washing speed is 600 r / min. At a solid-liquid ratio of 1:1 g / mL, the removal rates of K and Na are 39.8% and 52.9%, respectively, and the alumina content is 65.9%. At a solid-liquid ratio of 1:3 g / mL, the removal rates of K and Na are 50.8% and 70.1%, respectively, and the alumina content is 70.8%. At a solid-liquid ratio of 1:5 g / mL, the removal rates of K and Na are 54.1% and 74.7%, respectively, and the alumina content is 74.0%.
[0059] Decreasing the solid-liquid ratio from 1:1 g / mL to 1:3 g / mL had a significant impact on the removal rates of K and Na. This is mainly because the reduction in the solid-liquid ratio effectively lowers the viscosity of the material, facilitating thorough contact and mixing with the secondary aluminum ash and improving the removal rates of alkali metals K and Na. Furthermore, the reduced solid-liquid ratio also lowers the pH of the washing solution, reducing the OH- ions. - The concentration of K and Na was reduced, inhibiting their reaction with AlN and minimizing aluminum loss during washing. Further reducing the solid-liquid ratio to 1:5 g / mL resulted in maximum removal rates of K and Na (54.1% and 74.7%, respectively), and alumina content also reached its maximum (74.0%). With decreasing the solid-liquid ratio, other salts besides soluble salts, such as Na₃AlF₆ and CaF₂, remained poorly soluble in water, while the removal rates of K and Na and alumina content did not significantly improve. Furthermore, a lower solid-liquid ratio increases water consumption, wastewater treatment volume, and equipment load, increasing the treatment burden and operating costs. Therefore, a solid-liquid ratio of 1:3 g / mL was chosen as the optimal ratio for subsequent studies.
[0060] (4) Effect of water washing speed on element removal rate and alumina content
[0061] The preferred washing time is 3 hours, the preferred washing temperature is 60℃, and the preferred solid-liquid ratio is 1:3 g / mL. At a washing speed of 200 r / min, the removal rates of K and Na are 46.5% and 67.6%, respectively, and the alumina content is 71.4%. At a washing speed of 600 r / min, the removal rates of K and Na are 50.9% and 70.2%, respectively, and the alumina content is 70.1%. At a washing speed of 1000 r / min, the removal rates of K and Na are 52.8% and 71.0%, respectively, and the alumina content is 68.4%.
[0062] Example 2: Secondary aluminum ash washing experiment under optimal conditions
[0063] (1) Stability washing experiment under optimal washing parameters
[0064] Example 1 determined the optimal wet washing parameters: washing temperature 60℃, washing time 3h, solid-liquid ratio 1:3g / mL, and stirring speed 600r / min. A secondary wet washing stability experiment of aluminum ash was conducted under these conditions. Figure 4 As shown, the removal effects of K and Na elements are significant and stable, with a K removal rate of approximately 50% and a Na removal rate of approximately 70%. The average Al2O3 content in the secondary aluminum ash washing samples remained at around 71%. Overall, the factors affecting the removal rates of K and Na elements are: solid-liquid ratio > washing temperature > washing time > stirring speed.
[0065] (2) The effect of the washing process on the removal rate of F and Cl
[0066] The concentrations of fluorine and chlorine in the leaching solution of the secondary aluminum ash raw material were 3.73 mg / L and 1138.9 mg / L, respectively. In the leaching solution of the washed secondary aluminum ash sample, the concentrations of fluorine and chlorine decreased to 3.07 mg / L and 9.09 mg / L, respectively. The mass concentrations of fluorine and chlorine in the secondary aluminum ash raw material were 0.07 mg / kg and 30.52 mg / kg, respectively. In the washed secondary aluminum ash sample, the mass concentrations of fluorine and chlorine decreased to 0.06 mg / kg and 0.29 mg / kg, respectively. After water washing treatment, the contents of fluorine and chlorine both reached the national limits, and the removal rates of fluorine and chlorine reached 17.58% and 99.0%, respectively. Figure 5 As shown.
[0067] The wet washing method for secondary aluminum ash in this invention is a low-cost process that can remove harmful impurities, improve the efficiency of subsequent processing, and has a wide range of applications. This method can be used alone or in combination with high-temperature calcination. Based on the experimental process and test results of Examples 1-2, the optimal parameters for the wet washing method of this invention are: washing temperature 60℃, washing time 3h, solid-liquid ratio 1:3g / mL, and stirring speed 600r / min.
[0068] Example 3: Effect of ammonium chloride solution on element removal rate and alumina content
[0069] Under the optimal wet washing parameters of step (1) in Example 2, a washing experiment was conducted using ammonium chloride solution. When the ammonium chloride solution concentration was 5%, the removal rates of K and Na were 50.6% and 70.2%, respectively, and the alumina content was 75.3%. When the ammonium chloride solution concentration was 15%, the removal rates of K and Na were 51.7% and 71.1%, respectively, and the alumina content was 82.6%. When the ammonium chloride solution concentration was 20%, the removal rates of K and Na were 49.8% and 68.3%, respectively, and the alumina content was 84.1%. Figure 6 As shown.
[0070] When the concentration of ammonium chloride solution is increased to 20%, although the alumina content increases, it is only by about 2%. The removal rates of alkali metals K and Na do not increase but instead decrease slightly. This change may be related to the increase in chloride ion concentration in the solution. The increase in chloride ion concentration will hinder the further dissolution of chloride salts and reduce their solubility in the solution. However, the alumina content in the washing product only increases by about 2%, and the increase in content is not significant. Therefore, on the basis of ensuring the removal rate of alkali metals K and Na and increasing the alumina content, a 15% ammonium chloride solution can be selected as the washing solution.
[0071] Example 4: Optimization of high-temperature calcination process parameters for secondary aluminum ash
[0072] (1) Effect of calcination temperature on element removal rate and alumina content
[0073] The secondary aluminum ash washed under optimal washing parameters in step (1) of Example 2 was subjected to a calcination experiment. Under the conditions of a heating rate of 6℃ / min, a gas flow rate of 4L / min, and a holding time of 2h, the removal rates of K and Na were 10.70% and 16.8% respectively, and the alumina content was 78.2% at a calcination temperature of 700℃; the removal rates of K and Na were 40.3% and 42.9% respectively, and the alumina content was 84.2% at a calcination temperature of 1300℃; and the removal rates of K and Na were 42.2% and 45.1% respectively, and the alumina content was 85.9% at a calcination temperature of 1500℃.
[0074] Depend on Figure 3 XRD pattern analysis: At 1300℃, the diffraction peaks were mainly Al2O3 and MgAl2O4. The main components of the calcined high-alumina refractory material are Al2O3 and MgAl2O4, indicating that high-temperature calcination can help remove impurity elements and improve the quality of high-alumina refractory materials.
[0075] (2) Effect of calcination time on element removal rate and alumina content
[0076] The secondary aluminum ash washed under optimal washing parameters in step (1) of Example 2 was subjected to a calcination experiment. Under the conditions of a heating rate of 6℃ / min, a gas flow rate of 4L / min, and a preferred calcination temperature of 1300℃, the removal rates of K and Na were 30.3% and 36.5% respectively, and the alumina content was 83.4% after calcination for 1 h; the removal rates of K and Na were 43.0% and 45.4% respectively, and the alumina content was 88.2% after calcination for 4 h; and the removal rates of K and Na were 43.5% and 46.2% respectively, and the alumina content was 88.3% after calcination for 5 h.
[0077] Theoretically, higher temperatures yield better results. However, experimental results show that at a roasting temperature of 1500℃ compared to 1300℃, the removal rates of alkali metals K and Na, as well as the alumina content, were not significantly improved. Extending the roasting time from 4 hours to 5 hours did not significantly improve the removal of alkali metals K and Na, nor the alumina content. In a system where various components coexist, the mixing of multiple substances leads to a lower melting and boiling point than the pure substances. At high temperatures, some crystals will decompose successively, which is beneficial for element removal. However, considering that at excessively high temperatures, the melting of Al fills the gaps between particles, making the secondary aluminum ash denser, and the rapidly formed dense oxide layer of AlN also hinders the volatilization of salts such as NaCl and KCl, excessively long roasting times increase energy consumption and cost. Therefore, the high-temperature roasting treatment method for secondary aluminum ash in this invention can be derived from the experimental process and test results of Example 4. The optimal parameters for high-temperature roasting in this invention are: roasting temperature 1300℃, roasting time 4 hours.
[0078] Example 5
[0079] The optimal parameters for the combined wet washing and high-temperature calcination method for secondary aluminum ash obtained through Examples 1-4 can save costs, reduce energy consumption, and achieve resource utilization of secondary aluminum ash. The optimal washed sample of secondary aluminum ash obtained under the optimal washing parameters in Example 2 was applied to the calcination experiment of secondary aluminum ash. Under the optimal calcination parameters in Example 4, a high-alumina refractory material with alumina and magnesium aluminum spinel as the main components was calcined.
[0080] The material prepared in this embodiment has an alumina content of ≥88%, which meets the requirement of alumina content (≥80%) in the LZ-80 physicochemical index of GB / T 2988-2012; the K2O content is 0.06%, which meets the limit of potassium oxide (K2O) content ≤0.5% in high-alumina refractory materials; the Na2O content is 0.28%, which meets the limit of sodium oxide (Na2O) content ≤0.3% in high-alumina refractory materials; and the fluorine and chlorine contents have reached the limits specified in the implementation standard of GB5085.3-2007 "Identification Standard for Hazardous Waste - Leaching Toxicity Identification".
Claims
1. A method for combined treatment of secondary aluminum ash by wet washing and high-temperature calcination, characterized in that, Includes the following steps: (1) Pretreatment Secondary aluminum ash is obtained by sieving and dry ball milling to obtain secondary aluminum ash with uniform particle size. (2) Wet washing The secondary aluminum ash obtained in step (1) is mixed with water washing solution and washed to obtain a secondary aluminum ash water washing sample; The washing solution is an aqueous solution of ammonium chloride; the mass fraction of the ammonium chloride aqueous solution is 5-20%. The solid-liquid ratio of secondary aluminum ash to water washing solution was 1:3, g / mL; the water washing temperature was 60℃; the water washing time was 3h; and the water washing stirring speed was 600r / min. (3) High-temperature roasting The secondary aluminum ash water-washed sample obtained in step (3) was subjected to high-temperature calcination to obtain high-alumina refractory material; The high-temperature roasting temperature is 700~1500℃, and the roasting time is 1~5h.
2. The method for combined treatment of secondary aluminum ash by wet washing and high-temperature roasting as described in claim 1, characterized in that, In step (1), sieving refers to passing the secondary aluminum ash through a 60-mesh standard sieve; the rotation speed of the ball mill in the dry ball mill is controlled at 200~400 r / min, and the time is controlled at 10~60 min.
3. The method for combined treatment of secondary aluminum ash by wet washing and high-temperature roasting as described in claim 1, characterized in that, In step (3), the roasting temperature is 1300℃ and the roasting time is 4h.
4. The method for combined treatment of secondary aluminum ash by wet washing and high-temperature roasting as described in claim 1, characterized in that, In step (3), the roasting atmosphere is air, and the gas flow rate is 4L / min.
Citation Information
Patent Citations
Efficient and clean secondary aluminum ash harmless disposal method
CN110548753A
A method for recycling secondary aluminum ash
CN116462215B
A method for the combined treatment of secondary aluminum ash by ball milling separation, low-temperature roasting and water washing and leaching
CN116809604B
Resource utilization method of secondary aluminum ash
CN117800358A
Method for efficiently and harmlessly treating secondary aluminum ash
CN118341796A