A PVC pipe, its preparation method and application

By using an inner and outer layer composite structure and additives, the problems of insufficient wear resistance and heat deformation resistance of PVC pipes are solved, thereby improving the wear resistance and deformation resistance of PVC pipes when transporting liquids and extending their service life.

CN119192745BActive Publication Date: 2026-11-10RIFENG ENTERPRISE FOSHAN CO LTD +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411221393.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2026-11-10
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing PVC pipes generally have poor wear resistance, low Vicat softening temperature, and are prone to deformation at high temperatures. They are also prone to breakage and cracking when conveying liquids containing waste slag and excrement, making maintenance troublesome.

Method used

The inner and outer layers are composite structures. The inner layer contains polyvinyl chloride resin, stabilizer, calcium carbonate, lubricant, titanate coupling agent and other components, while the outer layer contains polyvinyl chloride resin, titanium dioxide, ABS resin and other components. The PVC pipe is prepared by co-extrusion molding. The inner and outer layers have good compatibility and no intermediate adhesive layer is required. Additives such as silica and polymethyl methacrylate are added to improve wear resistance and heat deformation resistance.

Benefits of technology

It significantly improves the wear resistance and heat deformation resistance of PVC pipes, reduces the risk of wear when transporting liquids, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119192745B_ABST
    Figure CN119192745B_ABST
Patent Text Reader

Abstract

This invention discloses a PVC pipe, its preparation method, and its applications, belonging to the field of plastic pipe technology. It includes an inner layer and an outer layer. The inner layer comprises the following components by weight: 100 parts polyvinyl chloride resin, 4-5 parts stabilizer, 5-8 parts calcium carbonate, 0.6-1 part first lubricant, 0.2-0.6 parts second lubricant, 0.28-0.5 parts glyceryl monostearate, 15-35 parts additives, 1-1.5 parts titanate coupling agent, and 0.2-0.5 parts carbon black. The PVC pipe of this invention exhibits excellent wear resistance and heat deformation resistance. When fluid passes through the inner layer, the pipe is not easily damaged or deformed, and it has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of plastic pipe technology, specifically to a PVC pipe, its preparation method, and its application. Background Technology

[0002] PVC pipes are widely used in water supply, building drainage, sewage, chemical and other technical fields due to their low cost, ease of processing and strong corrosion resistance, high strength and rigidity.

[0003] However, most PVC pipes on the market have average wear resistance and low Vicat softening temperature. They are prone to wear and deformation at high temperatures when transporting fluids. When used outdoors to transport liquids containing waste slag from power plants, calcium carbide plants, lead mines and other industrial and mining enterprises, as well as excrement from livestock farming, the pipes are prone to damage, brittleness and deformation, requiring manual repair, which is quite troublesome.

[0004] Therefore, this application is submitted. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the existing technology and provide a PVC pipe, its preparation method and application, wherein the PVC pipe has excellent wear resistance and heat deformation resistance.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] A PVC pipe includes an inner layer and an outer layer, wherein the inner layer comprises the following components in parts by weight: 100 parts polyvinyl chloride resin, 4-5 parts stabilizer, 5-8 parts calcium carbonate, 0.6-1 part first lubricant, 0.2-0.6 parts second lubricant, 0.28-0.5 parts glyceryl monostearate, 15-35 parts additives, 1-1.5 parts titanate coupling agent, and 0.2-0.5 parts carbon black.

[0008] This invention creatively combines the above-mentioned raw materials to obtain a PVC pipe with excellent wear resistance and heat deformation resistance. When fluid passes through the inner layer, the pipe is not easily damaged or deformed.

[0009] As a preferred embodiment of the present invention, the outer layer comprises the following components in parts by weight: 100 parts polyvinyl chloride resin, 4-5 parts stabilizer, 5-8 parts calcium carbonate, 8-10 parts titanium dioxide, 0.5-1 part first lubricant, 0.3-0.8 parts second lubricant, 0.2-0.6 parts glyceryl monostearate, 1-1.5 parts titanate coupling agent, 15-35 parts additives, 0-12 parts ABS resin, 0.8-1 part compatibilizer, and 0.5-1 part carbon black.

[0010] The pipe of the present invention has good compatibility between the inner and outer layers, and there is adhesion between the inner and outer layers, eliminating the need for an intermediate adhesive layer, resulting in a PVC pipe with excellent wear resistance and heat deformation resistance of both inner and outer layers.

[0011] As a preferred embodiment of the present invention, the additive comprises the following components in parts by weight: 20-55 parts silica, 40-75 parts polymethyl methacrylate, 2-2.5 parts ethylene bis-stearamide, 1-1.5 parts zinc stearate, 1-1.5 parts calcium stearate, and 0.2-0.5 parts titanate coupling agent.

[0012] This invention significantly improves the wear resistance and heat deformation resistance of pipes by adding the aforementioned additives containing silica, polymethyl methacrylate, ethylene bis-stearamide, zinc stearate, calcium stearate, and titanate coupling agent. This reduces the risk of wear on the inner wall of the pipes when transporting liquids such as waste slag and excrement, and increases the service life of the pipes.

[0013] The inventors of this invention have discovered that the dosage and composition of the additives have a significant impact on the heat resistance and wear resistance of the pipe. By controlling the dosage within the range of this invention, the wear resistance and heat resistance are significantly improved. However, when the dosage of the additives deviates from the range of this invention, the wear resistance and heat resistance will decrease significantly. At the same time, the inventors of this invention have discovered that both silica and PMMA are indispensable. The present invention uses silica and PMMA in combination, and the combined effect of the two synergistically improves the wear resistance and heat resistance.

[0014] As a preferred embodiment of the present invention, the additive comprises the following components in parts by weight: 30-45 parts silica, 50-65 parts polymethyl methacrylate, 2-2.5 parts ethylene bis-stearamide, 1-1.5 parts zinc stearate, 1-1.5 parts calcium stearate, and 0.2-0.5 parts titanate coupling agent.

[0015] In a preferred embodiment of the present invention, the polymethyl methacrylate has a melt flow rate of 2.3–3.7 g / 10 min at 230°C / 3.8 kg; and / or

[0016] The silica has a particle size of 2000–4000 mesh.

[0017] The inventors of this invention have discovered that, in particular, using PMMA with a melt flow rate of 2.3 to 3.7 g / 10 min and 2000 to 4000 mesh silica can significantly improve wear resistance and resistance to heat deformation.

[0018] In a preferred embodiment of the present invention, the melting point of the first lubricant is 108-112°C, and the melting point of the second lubricant is 92-98°C.

[0019] In a preferred embodiment of the present invention, the first lubricant is PE wax and the second lubricant is Fischer-Tropsch wax.

[0020] In a preferred embodiment of the present invention, the melt flow rate of the ABS resin at 200°C / 10kg is 16-26 g / 10 min.

[0021] In a preferred embodiment of the present invention, the compatibilizer is maleic anhydride-grafted ABS.

[0022] In a preferred embodiment of the present invention, the stabilizer is a zinc-calcium stabilizer.

[0023] As a preferred embodiment of the present invention, the thickness ratio of the inner layer to the outer layer is (0.6~0.75):(0.25~0.4); the composite tube D75*4mm includes an inner layer and an outer layer; the thickness of the inner layer is 2~3mm, and the wall thickness of the outer layer is 1~2mm.

[0024] This invention also provides a method for preparing PVC pipe, comprising the following steps:

[0025] The components of the inner tube are mixed and stirred to obtain the inner layer mixture; the components of the outer tube are mixed and stirred to obtain the outer layer mixture.

[0026] After loading the above-mentioned inner layer compound and outer layer compound into the co-extrusion equipment, co-extrusion is performed. The extruded material is placed in the molding die to form a PVC pipe, which is then shaped, cooled, drawn, and cut to obtain the PVC pipe.

[0027] The present invention also provides an application of PVC pipe in the manufacture of drainage pipes.

[0028] The beneficial effects of the present invention are as follows: (1) The PVC pipe of the present invention has excellent wear resistance and heat deformation resistance. When the fluid passes through the inner layer, the pipe is not easily damaged or deformed, and has a wide range of application prospects; (2) By adding the additives containing silica, polymethyl methacrylate, ethylene bis-stearamide, zinc stearate, calcium stearate and titanate coupling agent, the present invention significantly improves the wear resistance and heat deformation resistance of the pipe, reduces the risk of wear on the inner wall of the pipe when transporting liquids such as waste slag and excrement, and increases the service life of the pipe. Attached Figure Description

[0029] Figure 1 This is a schematic diagram of the PVC pipe structure of the present invention.

[0030] The diagram is labeled: 1. Outer layer; 2. Inner layer. Detailed Implementation

[0031] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0032] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0033] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0034] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0035] The raw materials used in the examples and comparative examples are described below:

[0036] Polyvinyl chloride resin: Xinjiang Zhongtai, brand name PVCsg5.

[0037] Stabilizer: Zinc-calcium stabilizer, Guangdong Xinda, brand name QY-20318D.

[0038] First lubricant: PE wax, melting point 110℃, Qingdao Bonnie, grade BN110.

[0039] Second lubricant: Fischer-Tropsch wax, melting point 95℃, Shanxi Lu'an, grade LA-W95.

[0040] Glyceryl monostearate: Hangzhou Oil & Fat Chemical Co., Ltd.

[0041] Titanate coupling agent: Isopropyl tris(dioctylphosphoyloxy)titanate, Jinan Rongzheng Chemical, brand name KR-12.

[0042] Carbon black: Cabot, grade 250R.

[0043] Calcium carbonate: 1250 mesh, from Guangyuan, Jiangxi.

[0044] Titanium dioxide: Nanjing Titanium Dioxide, grade R950.

[0045] Compatibilizer: Maleic anhydride grafted ABS, Shenyang Ketong, KT-2.

[0046] PMMA-1: Arkema, grade V825, with a melt flow rate of 3.7 g / 10 min at 230℃ / 3.8 kg.

[0047] PMMA-2: Arkema, grade V405, with a melt flow rate of 2.3 g / 10 min at 230℃ / 3.8 kg.

[0048] PMMA-3: Arkema, grade V826, with a melt flow rate of 1.6 g / 10 min at 230℃ / 3.8 kg.

[0049] PMMA-4: Arkema, grade V920, with a melt flow rate of 8 g / 10 min at 230℃ / 3.8 kg.

[0050] Silica: 3000 mesh, Delan Chemical.

[0051] Ethylene bis-stearamide: Kao Corporation, brand name EB-FF.

[0052] Zinc stearate: Zhongshan Huamingtai.

[0053] Calcium stearate: Zhongshan Huamingtai.

[0054] ABS-1: Melt flow rate of 20g / 10min at 200℃ / 10kg, Jilin Petrochemical, grade 0215A.

[0055] ABS-2: Melt flow rate of 16 g / 10 min at 200℃ / 10 kg, Jilin Petrochemical, grade 9715A.

[0056] ABS-3: Melt flow rate of 26 g / 10 min at 200℃ / 10 kg, Jilin Petrochemical, grade 9815A.

[0057] ABS-4: Melt flow rate of 9 g / 10 min at 200℃ / 10 kg, Jilin Petrochemical, grade 9710A.

[0058] ABS-5: Melt flow rate of 35 g / 10 min at 200℃ / 10 kg, Jilin Petrochemical, grade 0215F.

[0059] Unless otherwise specified, all components and raw materials used in the embodiments and comparative examples of this invention are commercially available, and the same type of components and raw materials are used in each parallel experiment.

[0060] Additives 1-10

[0061] The formulations of additives 1 to 10 are shown in Table 1 (all figures in Table 1 are parts by weight).

[0062] The preparation methods of additives 1 to 10 all include the following steps: the raw materials are added to a low-speed mixer at 200 rpm / min and stirred for 20 minutes according to the proportion to obtain the additives.

[0063] Table 1

[0064]

[0065] Examples 1-10, Comparative Examples 1-4

[0066] Examples 1-10 and Comparative Examples 1-4 were used to investigate the effect of the inner layer formulation on performance. The formulations of Examples 1-10 and Comparative Examples 1-4 are shown in Table 2 (all figures are parts by weight).

[0067] The inner layer preparation methods for Examples 1-10 and Comparative Examples 1-4 are as follows:

[0068] The components of the inner layer tube are mixed and stirred to obtain the inner layer mixture; the inner layer mixture is extruded and shaped to obtain the inner layer.

[0069] Table 2

[0070]

[0071]

[0072] Performance tests of Examples 1-10 and Comparative Examples 1-4

[0073] Abrasion resistance: Using Jiangsu Mingzhu MZ-4602 abrasion tester, 9 flat sample plates (100×100×2mm) were prepared and tested for 15 minutes each.

[0074] Vicat softening temperature test method: GB / T8802-2001.

[0075] Table 3

[0076] Wear amount (g) Vicat softening temperature (°C) Example 1 1.2314 84.2 Example 2 1.0188 86.6 Example 3 1.2112 87.5 Example 4 1.2114 86.7 Example 5 1.1117 86.2 Example 6 1.1126 86.5 Example 7 1.2239 85.8 Example 8 1.1112 85.9 Example 9 1.2001 88.5 Example 10 1.2201 83.2 Comparative Example 1 1.3111 88.9 Comparative Example 2 1.3221 88.1 Comparative Example 3 1.7564 81.4 Comparative Example 4 1.3455 88.3

[0077] As can be seen from Table 3, as the amount of wear-resistant agent increases, the Vicat softening point of the material increases slightly, while the amount of wear decreases slightly.

[0078] Examples 11-17

[0079] Examples 11-17 investigated the effect of the outer layer formulation on performance. The formulations of Examples 11-17 are shown in Table 4 (all figures are parts by weight).

[0080] The outer layer preparation method in Examples 11-17 is as follows:

[0081] The components of the outer layer tube are mixed and stirred to obtain the inner layer mixture; the outer layer mixture is extruded and shaped to obtain the outer layer.

[0082] Table 4

[0083]

[0084] Abrasion resistance: Using Jiangsu Mingzhu MZ-4602 abrasion tester, 9 flat sample plates (100×100×2mm) were prepared and tested for 15 minutes each.

[0085] Vicat softening temperature:

[0086] Table 5

[0087]

[0088]

[0089] As can be seen from Table 5, the outer layer formulation of the present invention has excellent wear resistance and excellent resistance to heat deformation.

[0090] Example 18

[0091] like Figure 1 As shown, Example 2 is used as the inner layer formula and Example 13 is used as the outer layer formula. The thickness ratio is 0.7:0.3 and the total thickness is 4mm. The above inner layer mixture and outer layer mixture are loaded into a co-extrusion device and co-extruded. The extruded material is placed in a molding die to form, and after shaping, cooling, traction and cutting, a PVC pipe is obtained.

[0092] Abrasion resistance: Using Jiangsu Mingzhu MZ-4602 abrasion tester, 9 flat sample plates (100×100×2mm) were prepared and tested for 15 minutes each, with 3 groups tested.

[0093] Vicat softening temperature: GB / T8802-2001.

[0094] Tensile strength: GB / T8804.2-2003.

[0095] Elongation at break: GB / T8804.1-2003.

[0096] Longitudinal shrinkage rate: GB / T6671-2001.

[0097] Table 6

[0098]

[0099] It is evident that the PVC pipe described in this invention possesses excellent wear resistance, heat deformation resistance, and mechanical properties, and has broad application prospects.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A PVC pipe, characterized in that, It includes an inner layer and an outer layer. The inner layer comprises the following components in parts by weight: 100 parts polyvinyl chloride resin, 4-5 parts stabilizer, 5-8 parts calcium carbonate, 0.6-1 part first lubricant, 0.2-0.6 parts second lubricant, 0.28-0.5 parts glyceryl monostearate, 15-35 parts additives, 1-1.5 parts titanate coupling agent, and 0.2-0.5 parts carbon black; The additive comprises the following components in parts by weight: 30-45 parts silica, 50-65 parts polymethyl methacrylate, 2-2.5 parts ethylene bis-stearamide, 1-1.5 parts zinc stearate, 1-1.5 parts calcium stearate, and 0.2-0.5 parts titanate coupling agent. The polymethyl methacrylate is manufactured by Arkema and its brand name is V825 or V405. The outer layer comprises the following components in parts by weight: 100 parts polyvinyl chloride resin, 4-5 parts stabilizer, 5-8 parts calcium carbonate, 8-10 parts titanium dioxide, 0.5-1 part first lubricant, 0.3-0.8 parts second lubricant, 0.2-0.6 parts glyceryl monostearate, 1-1.5 parts titanate coupling agent, 15-35 parts additives, 0-12 parts ABS resin, 0.8-1 part compatibilizer, and 0.5-1 part carbon black; The silica has a particle size of 2000~4000 mesh.

2. The PVC pipe according to claim 1, characterized in that, The melting point of the first lubricant is 108~112℃, and the melting point of the second lubricant is 92~98℃.

3. The PVC pipe according to claim 1, characterized in that, The melt flow rate of the ABS resin at 200°C / 10kg is 16~26g / 10min.

4. The PVC pipe according to claim 1, characterized in that, The compatibilizer is maleic anhydride-grafted ABS.

5. The method for preparing the PVC pipe according to any one of claims 1 to 4, characterized in that, Includes the following steps: The components of the inner tube are mixed and stirred to obtain the inner layer mixture; the components of the outer tube are mixed and stirred to obtain the outer layer mixture. After loading the above-mentioned inner layer compound and outer layer compound into the co-extrusion equipment, co-extrusion is performed. The extruded material is placed in the molding die to form a PVC pipe, which is then shaped, cooled, drawn, and cut to obtain the PVC pipe.

6. The use of the PVC pipe according to any one of claims 1 to 4 in the manufacture of drainage pipes.

Citation Information

Patent Citations

  • Polyvinyl chloride wear-resistant drain pipe as well as preparation method and application thereof

    CN115339162A