Cobalt-composite Prussian blue aqueous sodium-ion battery cathode material and its preparation method
By combining cobalt with Prussian blue materials, a high-efficiency cobalt-composite Prussian blue aqueous sodium-ion battery cathode material was prepared, which solved the problems of high water content, low specific capacity and rate performance of Prussian blue materials in aqueous sodium-ion batteries, and realized the high efficiency improvement and large-scale production application of the material.
Patent Information
- Application Number
- CN202411384655.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Existing Prussian blue materials have high water content and low specific capacity and rate performance in aqueous sodium-ion batteries, making it difficult to meet the needs of practical applications.
By using cobalt-based Prussian blue composite materials and controlling the cobalt content to prepare CoMnHCF materials, and combining them with conductive agents and binders, a high-efficiency cobalt-based Prussian blue aqueous sodium-ion battery cathode material was prepared.
It significantly improves the specific capacity and rate performance of the material, reduces the water content, is suitable for large-scale production, and has low cost and simple process.
Smart Images

Figure CN119252913B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aqueous sodium-ion battery technology, specifically to a cobalt-composite Prussian blue aqueous sodium-ion battery cathode material and its preparation method. Background Technology
[0002] With the rapid development of global industry and people's higher expectations for a better life, existing fossil fuels can no longer meet market demand. At the same time, the serious environmental pollution caused by fossil fuel combustion has prompted people to actively seek ways to replace fossil fuels with clean and renewable energy. However, clean and renewable energy is constrained by factors such as geographical conditions, climate change, and time, resulting in intermittent and random limitations. Therefore, the development of energy storage technology is particularly crucial. Among rechargeable batteries, lithium-ion batteries have been successfully applied in various portable electronic devices and electric vehicles due to their high energy density, long cycle life, and excellent rate performance. However, with the continuous expansion of energy storage scale, limited lithium resources, safety hazards such as flammability and explosiveness, and high prices make it difficult to meet energy storage needs. In contrast, sodium-ion batteries, due to their abundant resources, wide distribution, and similar physicochemical properties to lithium, have become the most promising partial alternative to lithium-ion batteries. Among them, aqueous sodium-ion batteries have attracted much attention due to their high energy density, low cost, and safety and environmental friendliness. Prussian blue materials, due to their open framework structure, efficient and simple synthesis methods, and low cost, have become widely used cathode materials. However, this material suffers from high water content, low specific capacity, and low rate performance, which greatly affects its practical application.
[0003] In existing technologies, there are two main methods to reduce the moisture content of Prussian blue materials. One is heating, which evaporates the moisture, but temperature control is challenging; too low a temperature makes it difficult to remove moisture effectively, while too high a temperature damages the material structure. The other method is ball milling, which yields highly crystalline materials, but the particle size and morphology are difficult to control precisely, thus affecting specific capacity and rate performance. Therefore, synthesizing Prussian blue cathode materials suitable for aqueous sodium-ion batteries with low water content and high specific capacity and rate performance remains a critical technical challenge. Summary of the Invention
[0004] The present invention aims to provide a cobalt-composite Prussian blue aqueous sodium-ion battery cathode material and its preparation method, so as to reduce the water content of the material and improve its specific capacity and rate performance.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: a cobalt-composite Prussian blue aqueous sodium-ion battery cathode material, comprising an electrode active material, a conductive agent and a binder, wherein the mass ratio is 7:2:1, and the electrode active material is CoMnHCF Prussian blue material.
[0006] Preferably, the preparation method of CoMHCF Prussian blue material includes the following steps:
[0007] S1: Weigh out a certain amount of manganese metal salt and cobalt metal salt respectively, dissolve them in 20-200mL of deionized water to form solution A, wherein the molar ratio of manganese metal salt to cobalt metal salt is (0.1-9):1;
[0008] S2: Weigh out a certain amount of transition metal salt b and sodium salt respectively, and dissolve them in 20-200 mL of deionized water to form solution B, wherein the molar ratio of transition metal salt b to sodium salt is 0.01-0.1;
[0009] S3: Slowly add solution A from S1 to solution B from S2 while stirring continuously. After all solution A has been added to solution B, continue stirring for 10-60 minutes, and then age for 1-24 hours.
[0010] S4: After the aging treatment, CoMnHCF Prussian blue material is obtained by centrifugation, washing, vacuum drying and grinding.
[0011] Preferably, the concentration of the manganese and cobalt metal salt mixture in S1 is 0.01-2 mol / L.
[0012] Preferably, the concentration of sodium salt in S2 is 0.001-3 mol / L.
[0013] Preferably, the concentration of transition metal salt b in S2 is 0.01-1 mol / L.
[0014] Preferably, the manganese metal salt in S1 is any one or a combination of several of MnCl2, Mn(NO3)2, MnSO4, and Mn(CH3COO)2.
[0015] Preferably, the cobalt metal salt in S1 is any one or a combination of several of CoSO4, Co(NO3)2, Co(CH3COO)2, and CoCl2.
[0016] Preferably, the transition metal salt b in S2 is any one of Na4Mn(CN)6, Na4Fe(CN)6, Na4Co(CN)6, Na4Ni(CN)6, Na4Cu(CN)6, and Na4Zn(CN)6.
[0017] Preferably, the vacuum drying temperature in S4 is 40-120℃, and the vacuum drying time is 10-24h.
[0018] This application also provides another technical solution, the preparation method of cobalt composite Prussian blue aqueous sodium-ion battery cathode material is as follows: CoMnHCF Prussian blue material, conductive agent and binder are weighed and mixed in a mass ratio of 7:2:1, and after thorough grinding, an appropriate amount of N-methylpyrrolidone is added as a solvent, and after stirring evenly, a uniform slurry is obtained. The slurry is coated on carbon cloth and placed in a vacuum drying oven at 40-120℃ for drying for 10-24 hours to obtain cobalt composite Prussian blue aqueous sodium-ion battery cathode material.
[0019] Compared with the existing technology, the beneficial technical effects of this technical solution are as follows:
[0020] (1) The cobalt-coated Prussian blue aqueous sodium-ion battery cathode material provided by this technical solution is prepared by partially replacing manganese with cobalt in MnHCF Prussian blue material and controlling the content of cobalt source. CoMnHCF-50 is rich in sodium and its phase structure is transformed into a sodium-rich monoclinic phase, which significantly improves the specific capacity. The specific capacity reaches 115.8 mAh / g at a current density of 300 mA / g.
[0021] (2) The cobalt-composite Prussian blue aqueous sodium-ion battery cathode material provided in this technical solution is a sodium-rich material with reduced vacancy numbers, which helps to reduce water content, thereby providing Na+. + Providing more storage sites and larger ion channels, aqueous sodium-ion batteries made using such materials as positive electrode active materials have better specific capacity and rate performance.
[0022] (3) The preparation method of the cobalt composite Prussian blue aqueous sodium-ion battery cathode material provided by this technical solution is efficient, safe and simple. The raw materials used are simple and readily available, the production cost is low and the process is simple, making it suitable for large-scale production. Attached Figure Description
[0023] Figure 1 The images show the XRD patterns of CoMnHCF-50, CoMnHCF-30, CoMnHCF-70, MnHCF, and CoHCF prepared in Examples 1-3 and Comparative Examples 1-2 of this invention.
[0024] Figure 2 The above are charge-discharge curves of the cobalt-composite Prussian blue aqueous sodium-ion battery cathode materials prepared in Examples 1-3 and Comparative Examples 1-2 of this invention.
[0025] Figure 3 Thermogravimetric analysis (TGA) diagrams of CoMnHCF-50 and MnHCF prepared in Example 1 and Comparative Example 1 of this invention;
[0026] Figure 4The graphs show the rate performance test results of CoMnHCF-50 and MnHCF prepared in Example 1 and Comparative Example 1 of this invention. Detailed Implementation
[0027] The following detailed description illustrates the specific implementation method:
[0028] Example 1
[0029] The cobalt-Prussian blue aqueous sodium-ion battery cathode material comprises an electrode active material, a conductive agent, and a binder, with a mass ratio of 7:2:1. The electrode active material is CoMnHCF Prussian blue, the conductive agent is carbon black, and the binder is polyvinylidene fluoride.
[0030] The preparation method of CoMnHCF Prussian blue material includes the following steps:
[0031] S1: Weigh out a certain amount of manganese metal salt and cobalt metal salt respectively, and dissolve them in 20-200 mL of deionized water to form solution A. The molar ratio of manganese metal salt to cobalt metal salt is (0.1-9):1, and the concentration of the mixed solution of manganese metal salt and cobalt metal salt is 0.01-2 mol / L. The manganese metal salt is any one or a combination of several of MnCl2, Mn(NO3)2, MnSO4, and Mn(CH3COO)2, and the cobalt metal salt is any one or a combination of several of CoSO4, Co(NO3)2, Co(CH3COO)2, and CoCl2. In this example, weigh out 3.2 mmol of manganese chloride tetrahydrate and 3.2 mmol of cobalt chloride hexahydrate, and dissolve them in 50 mL of deionized water. Stir thoroughly to form solution A. The concentration of the mixed solution of manganese chloride tetrahydrate and cobalt chloride hexahydrate in S1 is 0.128 mol / L.
[0032] S2: Weigh out a certain amount of transition metal salt b and sodium salt respectively, and dissolve them in 20-200 mL of deionized water to form solution B. The molar ratio of transition metal salt b to sodium salt is 0.01-0.1, the concentration of sodium salt is 0.001-3 mol / L, and the concentration of transition metal salt b is 0.01-1 mol / L. Transition metal salt b is any one of Na4Mn(CN)6, Na4Fe(CN)6, Na4Co(CN)6, Na4Ni(CN)6, Na4Cu(CN)6, and Na4Zn(CN)6. Sodium salt is any one or a combination of several of NaCl, Na2SO4, NaNO3, and CH3COONa. In this example, 14 g of sodium chloride and 1.42 g of sodium ferrocyanide are dissolved in 100 mL of deionized water and stirred thoroughly to form solution B. The concentration of sodium chloride is 2.4 mol / L, and the concentration of sodium ferrocyanide is 0.0467 mol / L.
[0033] S3: Slowly add solution A from S1 to solution B from S2. Stir continuously with a magnetic stirrer at 25°C. After all solution A has been added to solution B, continue stirring for 10-60 minutes, and then age the resulting suspension for 1-24 hours. In this embodiment, the stirring time is 15 minutes and the aging time is 2 hours.
[0034] S4: After the aging treatment, the product is separated by centrifugation and washed three times with a washing solvent. The obtained product is placed in a vacuum oven and dried at 40-120℃ for 10-24 hours. After thorough grinding, CoMnHCF Prussian blue material is obtained and named CoMnHCF-50 material. The washing solvent is any one or a combination of deionized water, ethanol, and acetone. In this embodiment, deionized water is selected as the washing solvent, the drying temperature is 60℃, and the drying time is 18 hours.
[0035] The preparation method of cobalt-composite Prussian blue aqueous sodium-ion battery cathode material is as follows: CoMnHCF Prussian blue material, conductive agent and binder are weighed and mixed in a mass ratio of 7:2:1, and after thorough grinding, an appropriate amount of N-methylpyrrolidone is added as a solvent. After stirring evenly, a uniform slurry is obtained. The slurry is evenly coated on the pre-treated carbon cloth and placed in a vacuum drying oven at 40-120℃ for 10-24 hours to obtain the cobalt-composite Prussian blue aqueous sodium-ion battery cathode material. In this embodiment, the conductive agent is carbon black, the binder is polyvinylidene fluoride, the amount of conductive agent is 5.7 mg, the amount of binder is 2.9 mg, the amount of CoMnHCF Prussian blue material is 20 mg, the amount of N-methylpyrrolidone is 400 μL, the drying temperature is 60℃, and the drying time is 12 hours.
[0036] The electrochemical performance was tested under the following conditions: at 25°C, the constant current charge-discharge test of the battery was conducted using a LANHECT2001A battery testing system, with the test voltage window set to 0-1.2V and the current density to 300-2000 mA / g. The test conditions for Examples 1-3 and Comparative Examples 1-2 were the same.
[0037] Example 2
[0038] Unlike Example 1, in the preparation method of CoMnHCF Prussian Blue material, in S1, 4.48 mmol of manganese chloride tetrahydrate and 1.92 mmol of cobalt chloride hexahydrate are dissolved in 50 mL of deionized water and stirred thoroughly to form solution A. The remaining steps are the same. In S4, CoMnHCF Prussian Blue material is obtained and named CoMnHCF-30.
[0039] Example 3
[0040] Unlike Example 1, in the preparation method of CoMnHCF Prussian Blue material, in S1, 1.92 mmol of manganese chloride tetrahydrate and 4.48 mmol of cobalt chloride hexahydrate are dissolved in 50 mL of deionized water and stirred thoroughly to form solution A. The remaining steps are the same. In S4, CoMnHCF Prussian Blue material is obtained and named CoMnHCF-70.
[0041] Comparative Example 1
[0042] Unlike Example 1, in the preparation method of CoMnHCF Prussian blue material, cobalt metal salt is not used in S1. 6.4 mmol of manganese chloride tetrahydrate is dissolved in 50 mL of deionized water and stirred thoroughly to form solution A. The remaining steps are the same. Prussian blue material is obtained in S4 and named MnHCF.
[0043] Comparative Example 2
[0044] Unlike Example 1, in the preparation method of CoMnHCF Prussian blue material, manganese metal salt is not used in S1. 6.4 mmol of cobalt chloride hexahydrate is dissolved in 50 mL of deionized water and stirred thoroughly to form solution A. The remaining steps are the same. Prussian blue material is obtained in S4 and named CoHCF.
[0045] The amounts of each component used in Examples 1-3 and Comparative Examples 1-2 are shown in Table 1:
[0046] Table 1
[0047] Dosage Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Molar amount of manganese chloride tetrahydrate (mmol / L) 3.2 4.48 1.92 6.4 0 Molar amount of cobalt chloride hexahydrate (mmol / L) 3.2 1.92 4.48 0 6.4 Concentration of solution A (mol / L) 0.128 0.128 0.128 0.128 0.128 Mass of sodium chloride (g) 14 14 14 14 14 Mass of sodium ferrocyanide (g) 1.42 1.42 1.42 1.42 1.42 Sodium chloride concentration (mol / L) 2.4 2.4 2.4 2.4 2.4 Concentration of sodium ferrocyanide (mol / L) 0.0467 0.0467 0.0467 0.0467 0.0467
[0048] XRD analysis was performed on the CoMnHCF-50, CoMnHCF-30, CoMnHCF-70, MnHCF, and CoHCF materials prepared in Examples 1-3 and Comparative Examples 1-2. The results are as follows: Figure 1 As shown. From Figure 1 As can be seen, the diffraction peaks of the CoMnHCF material after cobalt addition shift to a larger angle compared to MnHCF, indicating that the interplanar spacing is reduced, which is conducive to the rapid redox reaction of the transition metal in the material, thereby improving the rate performance. In addition, the crystal structure of CoMnHCF-30, CoMnHCF-50 and CoMnHCF-70 materials changes from the cubic phase of MnHCF to the sodium-rich monoclinic phase.
[0049] Charge-discharge tests were conducted on the cobalt-composite Prussian blue aqueous sodium-ion battery cathode materials prepared in Examples 1-3 and Comparative Examples 1-2, and the results are as follows: Figure 2 As shown in Table 2, Figure 2 Table 2 shows the specific capacity of Examples 1-3 and Comparative Examples 1-2 at a current density of 300 mA / g. From Table 2 and... Figure 2 It can be seen that before CoMnHCF-50 material, the first-cycle specific capacity increases with the increase of cobalt metal salt content. After CoMnHCF-50 material, the first-cycle specific capacity decreases with the increase of cobalt metal salt content. Therefore, the first-cycle specific capacity of CoMnHCF-50 material is optimal, and the specific capacity can reach 115.8mAh / g at a current density of 300mA / g.
[0050] Table 2
[0051] Testing items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Specific capacity (mAh / g) 115.8 100.5 108.2 35.4 107.4
[0052] The CoMnHCF-50 and MnHCF prepared in Example 1 and Comparative Example 1 were detected by inductively coupled plasma optical emission spectrometry (ICP-OES), and the results are shown in Table 3. From the data in Table 3, the molecular formulas of MnHCF and CoMnHCF-50 can be calculated as Na... 1.15 Mn[Fe(CN)6] 0.73 Na 1.79 Co 0.74 Mn 0.26 [Fe(CN)6] 0.82 As can be seen from the molecular formula, the Na content in CoMnHCF-50 is significantly increased, making it a sodium-rich material, which helps improve specific capacity. The reduced number of vacancies also helps reduce water content.
[0053] Table 3
[0054] Mass percentage (wt%) Na Mn Co Fe Comparative Example 1 (MnHCF) 9.701 20.222 15.044 Example 1 (CoMnHCF-50) 11.122 3.923 11.727 12.356
[0055] Thermogravimetric analysis (TGA) was performed on CoMnHCF-50 and MnHCF prepared in Example 1 and Comparative Example 1, and the results are as follows: Figure 3 As shown, from Figure 3 As can be seen, the water content (adsorbed water and lattice water) of CoMnHCF-50 is significantly reduced, which can help reduce the water content of Na. + Providing more storage sites and larger ion channels helps improve specific capacity and rate performance.
[0056] Rate performance tests were conducted on CoMnHCF-50 and MnHCF prepared in Example 1 and Comparative Example 1, and the results are as follows: Figure 4 As shown, from Figure 4 As can be seen, MnHCF is rapidly damaged in the first cycle, while CoMnHCF-50 has a higher rate performance of 73.2% at 2000mA / g.
[0057] The above descriptions are merely embodiments of the present invention, and common knowledge such as specific technical solutions and / or characteristics are not described in detail here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the technical solutions of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.
Claims
1. A cobalt-composite Prussian blue aqueous sodium-ion battery cathode material, characterized in that: The composition includes electrode active material, conductive agent, and binder in a mass ratio of 7:2:
1. The electrode active material is CoMnHCF-50 Prussian blue. The preparation method of CoMnHCF-50 Prussian blue material is also described. Includes the following steps: S1: Weigh out 3.2 mmol of manganese chloride tetrahydrate and 3.2 mmol of cobalt chloride hexahydrate and dissolve them in 50 mL of deionized water to form solution A. The concentration of the mixed solution of manganese chloride tetrahydrate and cobalt chloride hexahydrate in solution A is 0.128 mol / L. S2: Weigh out 14g of sodium chloride and 1.42g of sodium ferrocyanide and dissolve them in 100mL of deionized water to form solution B, so that the concentration of sodium chloride is 2.4mol / L and the concentration of sodium ferrocyanide is 0.0467mol / L. S3: Slowly add solution A from S1 to solution B from S2 while stirring continuously. After all solution A has been added to solution B, continue stirring for 15 minutes and then age for 2 hours. S4: After aging treatment, CoMnHCF-50 Prussian blue material is obtained by centrifugation, washing, vacuum drying, and grinding. The molecular formula of the CoMnHCF-50 material is Na. 1.79 Co 0.74 Mn 0.26 [Fe(CN)6] 0.82 It is a sodium-rich monoclinic phase.
2. The method for preparing the cobalt-composite Prussian blue aqueous sodium-ion battery cathode material according to claim 1, characterized in that: CoMnHCF-50 Prussian blue material, conductive agent, and binder were weighed and mixed in a mass ratio of 7:2:
1. After thorough grinding, an appropriate amount of N-methylpyrrolidone was added as a solvent and stirred evenly to obtain a uniform slurry. The slurry was then coated onto carbon cloth and placed in a vacuum drying oven at 40-120℃ for 10-24 hours to obtain a cobalt-composite Prussian blue aqueous sodium-ion battery cathode material.
Citation Information
Patent Citations
Sodium-ion battery Prussian blue positive electrode material and preparation method and application thereof
CN113526527A