Decorative piece

By introducing a textured surface and a specific combination of particle resins into the surface protective layer of the decorative sheet, the problems of wet touch and low gloss of the decorative sheet are solved, improving its durability and processability, and making it suitable for the manufacture of decorative panels on a variety of substrates.

CN119317538BActive Publication Date: 2026-11-17TOPPAN HOLDINGS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380044997.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-06-24
Filing Date
2023-06-22
Publication Date
2026-11-17
Estimated Expiration
2043-06-22

AI Technical Summary

Technical Problem

Existing decorative panels lack designs that give a wet-touch feel and are difficult to work with while maintaining a low gloss level.

Method used

The surface protective layer is formed by setting an uneven structure in the surface protective layer, combining particles of specific size and content with ionizing radiation-curable resin, to form a surface protective layer with a gloss of less than 10. The cross-sectional height difference Rdc/t of the uneven structure is 0.1 to 0.2, and the thickness is 2μm to 18μm.

Benefits of technology

It achieves a moist tactile experience on the surface of decorative panels while maintaining low gloss and good durability, and is suitable for the manufacture of decorative panels on a variety of substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119317538B_ABST
    Figure CN119317538B_ABST
Patent Text Reader

Abstract

A decorative sheet (1) comprises a raw material layer (2) and a surface protective layer (5) disposed on one surface of the raw material layer (2). The surface of the surface protective layer (5) is provided with an uneven structure comprising a plurality of ridges protruding in a ridge shape. The ratio of the cross-sectional height difference Rdc of the uneven structure of the surface protective layer (5) to the thickness t of the surface protective layer (5) is Rdc / t, which is more than 0.1 and less than 0.2. The thickness t of the surface protective layer (5) is more than 2 μm and less than 18 μm. The surface protective layer (5) contains a cured resin product and particles. The average particle size of the particles is more than 3 μm. The particles are contained in the surface protective layer (5) in an amount of more than 3 parts by mass and less than 11 parts by mass relative to 100 parts by mass of the resin. The gloss of the surface protective layer (5) is less than 10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to decorative sheets. Background Technology

[0002] Decorative panels are used to decorate the surfaces of interior and exterior materials such as doors, windows, furniture, building materials, and flooring, giving these components a sense of design and durability. Decorative panels are generally bonded to the surface of substrates such as wood, wood-based panels, metal sheets, non-combustible boards, paper substrates, and resin substrates using adhesives to create decorative panels, and are thus widely used.

[0003] Design elements can be incorporated, such as using various printing methods to create patterns like wood grain or stone texture. Decorative pieces are sometimes preferred in solid colors without patterns. The choice of whether or not to have patterns, and the type of pattern, varies greatly depending on the intended use and personal preference.

[0004] When it comes to the design of decorative panels, the surface gloss is also important. As decorative panels, depending on the purpose and preference, there are various options available, ranging from high gloss like a mirror to low gloss with no reflection at all.

[0005] In addition, as mentioned above, another important function of decorative panels, alongside design features, is durability. Durability refers to a comprehensive evaluation of resistance to damage, staining, and whether these properties can be ensured over a long period. Requirements vary depending on the environment and conditions in which the decorative panels are used, but high-performance decorative panels are always required.

[0006] To enhance durability, a protective coating is typically formed on the outermost surface of the decorative piece. Additionally, to adjust the gloss level, particularly to achieve a low-gloss finish, a gloss modifier (matte additive) is usually added to the protective coating.

[0007] Furthermore, in order to form decorative materials such as decorative panels, the decorative pieces are usually subjected to processes such as cutting or bending, so it is preferable to have processability that can withstand these processes.

[0008] Thus, as a decorative sheet that takes into account design (low gloss), scratch resistance, and stain resistance, there is, for example, the decorative sheet described in Patent Document 1.

[0009] Existing technical documents

[0010] Patent documents

[0011] Patent Document 1: Japanese Patent Application Publication No. 2019-119138 Summary of the Invention

[0012] The problem that the invention aims to solve

[0013] The purpose of this invention is to provide a decorative sheet that imparts a moist tactile feel.

[0014] Methods for solving problems

[0015] According to one aspect of the present invention, a decorative sheet is provided, comprising a raw material layer and a surface protective layer disposed on one surface of the raw material layer, wherein the surface of the surface protective layer is provided with an uneven structure comprising a plurality of ridges each projecting in a ridge-like manner, wherein the ratio of the cross-sectional height difference Rdc of the uneven structure of the surface protective layer to the thickness t of the surface protective layer, Rdc / t, is 0.1 or more and 0.2 or less, the thickness t of the surface protective layer is 2 μm or more and 18 μm or less, the surface protective layer contains a cured resin product and particles, wherein the average particle size is 3 μm or more, the particles are contained in the surface protective layer in an amount of 3 parts by mass or more and 11 parts by mass relative to 100 parts by mass of the resin, and the gloss of the surface protective layer is less than 10.

[0016] According to other aspects of the invention, a decorative sheet relating to the above aspects is provided, wherein the average particle size of the particles is 3 μm or more and 11 μm or less.

[0017] According to yet another aspect of the invention, a decorative sheet relating to any of the above aspects is provided, wherein the resin is an ionizing radiation-curing resin.

[0018] According to yet another aspect of the invention, a decorative sheet relating to any of the foregoing aspects is provided, wherein the resin is an acrylate.

[0019] According to yet another aspect of the invention, a decorative sheet is provided that relates to any of the above aspects, wherein the resin is a trifunctional acrylate comprising a repeating structure, wherein the repeating structure is repeated 3 times or more but less than 20 times.

[0020] According to yet another aspect of the invention, a decorative sheet is provided that relates to any of the above aspects, wherein the resin is a tetrafunctional acrylate containing repeating structures, the repeating structures being repeated 20 to 35 times.

[0021] According to yet another aspect of the invention, a decorative sheet relating to any of the above aspects is provided, wherein a pattern layer is further provided between the raw material layer and the surface protective layer.

[0022] According to another aspect of the present invention, a decorative material is provided, comprising: a decorative sheet according to any of the above aspects, and a substrate for attaching the decorative sheet.

[0023] The effects of the invention

[0024] According to the present invention, it is possible to provide a decorative sheet that imparts a moist tactile feel. Attached Figure Description

[0025] [ Figure 1 ] Figure 1 This is a cross-sectional view of a decorative material comprising a decorative sheet according to one embodiment of the present invention.

[0026] [ Figure 2 ] Figure 2 yes Figure 1 A cross-sectional view of the surface protective layer contained in the decorative piece.

[0027] [ Figure 3 ] Figure 3 This is a microscope image of the surface protective layer contained in a decorative sheet, which is an example of the present invention. Detailed Implementation

[0028] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. The embodiments described below are more specific embodiments of any of the above aspects. The matters described below may be incorporated into the above aspects individually or in combination.

[0029] Furthermore, the embodiments shown below illustrate configurations for embodying the technical concept of the present invention. The technical concept of the present invention is not limited by the material, shape, or structure of the constituent components described below. Various modifications can be made to the technical concept of the present invention within the scope defined by the claims.

[0030] It should be noted that for elements with the same or similar functions, the same reference numerals will be used in the accompanying drawings below, and repeated descriptions will be omitted. Furthermore, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in other directions, as well as the relationship between the dimensions of one component and the dimensions of other components, may differ from the actual situation.

[0031] <1> Decorative materials and decorative panels

[0032] Figure 1 This is a cross-sectional view of a decorative material comprising a decorative sheet according to one embodiment of the present invention. Figure 2 yes Figure 1 A cross-sectional view of the surface protective layer contained in the decorative piece. Figure 3 This is a microscope image of the surface protective layer contained in a decorative sheet, which is an example of the present invention.

[0033] It should be noted that, Figure 2 The cross-section shown is along the thickness direction of the surface protective layer. Additionally, Figure 3 The microscope images are planar images obtained using a laser microscope (Olympus Corporation OLS-4000).

[0034] Figure 1 The decorative material 11 shown includes a substrate B and a decorative sheet 1 adhered thereto. Here, the decorative material 11 is a decorative panel. The decorative panel can be flat, curved, or folded. The decorative material 11 can also have shapes other than a panel.

[0035] Here, substrate B is a board material. The board material can be, for example, wood-based panels, inorganic panels, metal panels, or composite panels made of multiple materials. Substrate B can also have shapes other than those of a board.

[0036] Decorative sheet 1 includes a base material layer 2, a pattern layer 3, a transparent resin layer 4, a surface protective layer 5, an adhesive layer 7, a primer layer 6, and a masking layer 8. The pattern layer 3, adhesive layer 7, transparent resin layer 4, and surface protective layer 5 are sequentially disposed on the side of the base material layer 2 opposite to the side facing the substrate B, starting from the base material layer 2 side. The masking layer 8 and primer layer 6 are sequentially disposed on the side of the base material layer 2 facing the substrate B, starting from the base material layer 2 side. One or more of the pattern layer 3, transparent resin layer 4, primer layer 6, adhesive layer 7, and masking layer 8 may be omitted. The elements included in decorative sheet 1 will be described sequentially below.

[0037] <1.1> Raw Material Layer

[0038] As the raw material layer 2 or its material, materials can be selected from paper, synthetic resin, foamed synthetic resin, rubber, nonwoven fabric, synthetic paper, metal foil, etc. Examples of paper include thin paper, titanium paper, resin-impregnated paper, etc. Examples of synthetic resins include polyethylene, polypropylene, polybutene, polystyrene, polycarbonate, polyester, polyamide, ethylene-vinyl acetate copolymer, polyvinyl alcohol, acrylic resins, etc. Examples of rubbers include ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, styrene-butadiene copolymer rubber, styrene-isoprene-styrene block copolymer rubber, styrene-butadiene-styrene block copolymer rubber, polyurethane, etc. Examples of nonwoven fabrics include organic or inorganic nonwoven fabrics. Examples of metals used as metal foils include aluminum, iron, gold, silver, etc.

[0039] Considering printability and cost, the thickness of the base material layer 2 is preferably in the range of 20μm to 250μm.

[0040] <1.2> Primer layer

[0041] When using an olefin-based resin as the material for the base layer 2, the surface of the base layer 2 is mostly inert. Therefore, in this case, it is preferable to provide a primer layer 6 between the base layer 2 and the substrate B. When the base layer 2 is made of an olefin-based material, in order to omit the primer layer 6 and improve the adhesion between the base layer 2 and the substrate B, the base layer 2 can also undergo surface modification treatments such as corona treatment, plasma treatment, ozone treatment, electron beam treatment, ultraviolet treatment, or dichromate treatment.

[0042] As the material for the primer layer 6, for example, the material of the pattern layer 3 described later can be used. Since the primer layer 6 is applied to the back side of the decorative sheet 1, when considering the winding of the decorative sheet 1 in a mesh shape, an inorganic filler can be added to the primer layer 6 to avoid adhesion and improve the adhesion to the adhesive. Examples of inorganic fillers include silica, aluminum oxide, magnesium oxide, titanium oxide, barium sulfate, etc.

[0043] <1.3> Concealment Layer

[0044] To provide concealment of the substrate B in the decorative sheet 1, a colored sheet can be used as the raw material layer 2, or an opaque concealing layer 8 can be provided. The concealing layer 8 can, for example, be made of the same material as the pattern layer 3 described later. However, since the concealing layer 8 is for concealment purposes, opaque pigments, titanium dioxide, iron oxide, etc., are preferably used as pigments. Furthermore, to improve concealment, metals such as gold, silver, copper, and aluminum can be added to the material of the concealing layer 8. Thin sheets of aluminum are typically added.

[0045] <1.4> Pattern Layer

[0046] Pattern layer 3 is a layer formed by printing a pattern onto the base material layer 2 using ink. As a binder for the ink, nitrocellulose, cellulose, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral, polyurethane, acrylics, polyesters, or their modified forms can be used alone or in combination. The binder can be water-based, solvent-based, or emulsion-type, and can be a one-component or a two-component type using a curing agent. Pattern layer 3 can be formed by curing the layer formed by curable ink using irradiation with ultraviolet light or an electron beam. The most common method is to use urethane-based inks and cure them with isocyanates. In addition to the binder, the ink used to form pattern layer 3 may contain pigments, dyes, colorants, extender pigments, solvents, and various additives commonly found in inks. Examples of versatile pigments include condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolide, cobalt, phthalocyanine, carbon, titanium dioxide, iron oxide, mica, and pearl pigments.

[0047] In addition to ink coating, the pattern layer 3 can also be designed by vapor deposition or sputtering of various metals. In particular, it is preferable to add a light stabilizer to the ink. This can suppress the deterioration of the decorative sheet 1 itself caused by the light degradation of the ink, and extend the life of the decorative sheet 1.

[0048] <1.5> Adhesive Layer

[0049] Adhesive layer 7 is also known as heat-sensitive adhesive layer, anchoring coating, or dry laminated adhesive layer.

[0050] There are no particular limitations on the resin material for the adhesive layer 7; for example, it can be appropriately selected and used from acrylic, polyester, polyurethane, epoxy, and other resin materials. Alternatively, an ethylene-vinyl acetate copolymer adhesive can also be used as the resin material for the adhesive layer 7. The coating method can be appropriately selected based on the viscosity of the adhesive. Typically, a gravure coating machine is used to form the adhesive layer 7 on top of the pattern layer 3, followed by laminating the transparent resin layer 4. It should be noted that if sufficient adhesive strength is obtained between the transparent resin layer 4 and the pattern layer 3, the adhesive layer 7 can be omitted.

[0051] <1.6> Transparent Resin Layer

[0052] As the resin material for the transparent resin layer 4, an olefin-based resin is preferably used. Examples of olefin-based resins, besides polypropylene, polyethylene, and polybutene, include α-olefins (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecanene, 1-hexadecene, 1-heptadecene, 1-heptadecene, 1-octadecene, 1-nonadecanene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-di ...hexene, 4,4-dimethyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-butene, 3-methyl-1-pentene, 3-methyl-1-pentene, 3-methyl-1-hexene, 3-methyl-1-pentene, 3-methyl-1-pentene, 3-methyl-1-hexene, 3-methyl-1-pentene, 3-methyl-1-hexene, 3-methyl-1-pentene, 3-methyl-1-pentene, 3-methyl-1-hexene, 3- Polymers obtained by homopolymerization or copolymerization of two or more of the following: 1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, etc.; copolymers obtained by copolymerizing ethylene or α-olefins with monomers other than those thereof, such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-butyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, etc.

[0053] Furthermore, to improve the surface strength of the decorative sheet 1, highly crystalline polypropylene is preferably used as the resin for the transparent resin layer 4. It should be noted that various additives, such as heat stabilizers, light stabilizers, anti-blocking agents, catalyst trapping agents, colorants, light scattering agents, and gloss modifiers, may be added to the transparent resin layer 4 as needed. As heat stabilizers, phenolic, sulfur-based, phosphorus-based, and hydrazine-based agents are generally added in any combination; as light stabilizers, hindered amine-based agents are generally added in any combination.

[0054] <1.7> Surface Protective Layer

[0055] The surface protective layer 5 includes a core 5A and a plurality of ridge-shaped portions 5B, each protruding in a ridge-like manner from one side of the core 5A. These ridge-shaped portions 5B form a concave-convex structure.

[0056] Here, in the decorative piece 1 according to this embodiment, "ridge-like" refers to a convex shape that is linear in plan view. The shape of the ridge portion 5B in plan view can be curved or straight, but from the viewpoint of the fingerprint resistance of the decorative piece 1, a curved shape is preferred. Each ridge portion 5B may or may not be branched in plan view. In addition, in this disclosure, the ridge portion 5B is, for example, the portion from the lowest part to the top part of the concave-convex shape provided on the surface of the surface protective layer 5, and the core portion 5A refers to the portion of the surface protective layer 5 other than the ridge portion 5B.

[0057] For example, such as Figure 3 As shown, each of the ridges 5B is curved, and at least a portion of them are adjacent in the width direction. At locations where at least a portion of the ridges 5B are adjacent in the width direction, the cross-section of the surface protective layer 5, parallel to both the width direction and the thickness direction of the surface protective layer 5, is as follows. Figure 2 As shown, the part with the concave-convex structure has a sinusoidal wave shape or other wave shape.

[0058] The ratio of the cross-sectional height difference Rdc of the uneven structure of the surface protective layer 5 to the thickness t of the surface protective layer 5, Rdc / t (hereinafter also referred to as "ratio Rdc / t"), is 0.1 to 0.2. Preferably, the ratio Rdc / t is 0.11 to 0.19.

[0059] "Sectional height difference Rdc" is a surface characteristic parameter specified in JIS B0601:2013. Rdc represents the difference in cross-sectional height of the roughness curve, indicating the steepness of the uneven shape. Here, the highest peak of the roughness curve is set as the reference for the cross-sectional height c. Furthermore, c(Rmr1) is set as the cross-sectional height when the load length ratio Rmr of the roughness curve is 10%, and c(Rmr2) is set as the cross-sectional height when the load length ratio Rmr of the roughness curve is 25%. The cross-sectional height difference Rdc (μm) of the roughness curve is the difference between the cross-sectional heights c(Rmr1) and c(Rmr2). When the cross-sectional height difference Rdc is divided by the thickness t of the surface protective layer 5 to obtain the ratio Rdc / t, the steepness of the uneven shape per unit thickness of the surface protective layer 5 can be represented.

[0060] It should be noted that the area on the surface of the protective layer corresponding to the portion where the load length ratio Rmr of the roughness curve is less than 10% is the area initially contacted by the fingertip when pressing the protective layer. The area on the surface of the protective layer where the fingertip initially contacts the protective layer has a relatively small impact on the wet feel. Furthermore, the area on the surface of the protective layer where the pressure applied from the fingertip is extremely high also has a small impact on the wet feel. However, when the pressure applied from the fingertip to the protective layer increases to a certain extent, the inclination of the area where the fingertip initially contacts the protective layer has a significant impact on the wet feel. This area corresponds to the portion on the surface of the protective layer where the load length ratio Rmr of the roughness curve is in the range of 10% to 25%.

[0061] When the value of Rdc / t is between 0.1 and 0.2, the slope of the uneven surface is relatively gentle. In this case, when pressing the surface of the decorative piece with a finger while sliding the finger across the surface, the indentation resistance caused by the contact between the finger and the surface is small, and the contact area between the finger and the raised surface gradually increases, thus obtaining a tactile sensation of the decorative piece adhering to the finger. This tactile sensation can be described as a "wet touch".

[0062] On the other hand, when Rdc / t is greater than 0.2, the slope of the uneven shape becomes steep. In this case, when pressing the surface of the decorative piece with a finger while sliding the finger across the surface, the pressure resistance caused by the contact between the finger and the surface is large, and the unevenness is felt. This tactile sensation can be described as a "rough" feel.

[0063] Furthermore, when Rdc / t is less than 0.1, the slope of the uneven surface is quite gentle. In this case, when pressing the surface of the decorative piece with a finger while sliding the finger across the surface, the indentation resistance caused by the contact between the finger and the surface is small, and the contact area between the finger and the raised surface is large from the beginning of the pressing action, and the increase of this contact area with the pressing action is quite slow. Therefore, in this case, a tactile sensation is obtained where the surface of the decorative piece adheres to the finger; on the other hand, because the slope of the uneven surface is quite gentle, a smooth sliding sensation is obtained compared to the aforementioned "wet sensation," and overall, the impression of a smooth sliding sensation is enhanced. This sensation can be described as a "smooth sensation."

[0064] The thickness t of the surface protective layer 5 is 2 μm to 18 μm. Preferably, the thickness t of the surface protective layer 5 is 3 μm to 10 μm. When the thickness of the surface protective layer 5 is increased, a tendency to increase the value of Rdc / t is observed. Therefore, when the thickness of the surface protective layer 5 is too small or too large, it is difficult to achieve a "wet feel." Furthermore, when the thickness of the surface protective layer 5 is reduced, it is difficult to achieve low gloss. Here, the thickness of the surface protective layer 5 is determined by observing a cross-section using a scanning electron microscope and averaging over 25 points. Specifically, the thickness of the surface protective layer 5 can be determined as described in the embodiments described later. It should be noted that when the coating liquid for the surface protective layer described later is solvent-free, the thickness of the coating film formed by the coating liquid for the surface protective layer is equal to the thickness of the surface protective layer 5.

[0065] The surface protective layer 5 contains the cured products and particles of the resin.

[0066] The resin contained in the surface protective layer 5 is preferably an ionizing radiation-curable resin. Here, "ionizing radiation" refers to a beam of charged particles such as an electron beam. The ionizing radiation-curable resin is cured by irradiation with ionizing radiation. Alternatively, the ionizing radiation-curable resin can also be cured by ultraviolet irradiation. The ionizing radiation-curable resin used here is cured by irradiation with light of wavelength below 200 nm, and on the other hand, it has a high absorption coefficient for this light.

[0067] The amount of cured product of the ionizing radiation-curable resin in the surface protective layer 5 is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. As the ionizing radiation-curable resin, various known resins such as monomers or commercially available oligomers can be used, for example, (meth)acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins. The ionizing radiation-curable resin can be either a water-based resin or a non-water-based (organic solvent-based) resin.

[0068] The main component of the ionizing radiation curable resin is preferably acrylate. Here, the main component of the ionizing radiation curable resin refers to the component that accounts for 60% or more by mass in the ionizing radiation curable resin. The ionizing radiation curable resin preferably contains acrylate in an amount of 70 parts by mass or more, more preferably in an amount of 80 parts by mass or more. The ionizing radiation curable resin is more preferably acrylate.

[0069] The acrylate is preferably a acrylate with two or more functional groups, more preferably a acrylate with three or more functional groups. In order to obtain a surface protective layer 5 with excellent scratch resistance, the acrylate is preferably three or more functional groups. There is no upper limit to the number of functional groups of the acrylate, but according to one example, it is six functional groups or less.

[0070] The acrylate preferably contains a repeating structure. This repeating structure is, for example, any one of an ethylene oxide (EO) structure, a propylene oxide (PO) structure, and an ε-caprolactone (CL) structure. The repeating structure is preferably ethylene oxide or propylene oxide. In the acrylate, the repeating structure may be located between an acryloyl group and a hydroxymethyl group in the ring-opening state.

[0071] The repetition rate of the repeating structure is preferably 3 or more. When using an acrylate with a high repetition rate, the cured film tends to expand inward during the first irradiation step described later, thus easily creating wrinkles on the coating surface corresponding to the ridge 5B. Furthermore, when using an acrylate with a high repetition rate, a tendency is observed for the value of Rdc / t to increase. However, as the repetition rate increases, the crosslinking density decreases, and the scratch resistance of the surface protective layer decreases.

[0072] In a preferred embodiment, the ionizing radiation-curable resin is a trifunctional acrylate containing a repeating structure. Examples of trifunctional acrylates containing a repeating structure include EO-modified, PO-modified, or CL-modified trimethylolpropane triacrylate, glycerol triacrylate, isocyanurate triacrylate, or pentaerythritol triacrylate. In the trifunctional acrylate containing a repeating structure, the number of repetitions is preferably 3 or more, more preferably 3 or more but less than 30, and even more preferably 3 or more but less than 20.

[0073] In another preferred embodiment, the ionizing radiation-curable resin is a tetrafunctional acrylate containing a repeating structure. The tetrafunctional acrylate containing the repeating structure is, for example, an EO-modified, PO-modified, or CL-modified pentaerythritol tetraacrylate. In the tetrafunctional acrylate containing the repeating structure, the number of repetitions is preferably 12 or more, more preferably 12 or more and 50 or less, further preferably 20 or more and 50 or less, and even more preferably 20 or more and 35 or less.

[0074] The number of repetitions of the above repeating structure can be analyzed using MALDI-TOF-MS. Ionizing radiation-cured resins sometimes exhibit molecular weight distributions. In the case of molecular weight distributions, the number of repetitions is set as the number of repetitions corresponding to the molecular weight with the strongest peak in the MALDI-TOF-MS mass spectrum.

[0075] The particles contained in the surface protective layer 5 can be, for example, particles made of organic materials such as polyethylene (PE) wax, polypropylene (PP) wax, and resin beads; or particles made of inorganic materials such as silicon dioxide, glass, alumina, titanium dioxide, zirconium oxide, calcium carbonate, and barium sulfate.

[0076] The average particle size (D50) is 3 μm or more. The average particle size (D50) is preferably 3 μm or more and 11 μm or less, more preferably 4 μm or more and 10 μm or less.

[0077] When the surface protective layer 5 contains particles, wrinkles can be generated more uniformly on the coating surface during the first irradiation process described later. When the average particle size (D50) increases, a tendency to decrease the value of Rdc / t can be observed. Therefore, when the average particle size (D50) is too small or too large, it is difficult to achieve a "wet feel." Furthermore, when using large particles, the particles can easily detach from the surface protective layer 5, making it difficult to achieve high scratch resistance. With small particles, the effect of uniformly generating wrinkles is minimal.

[0078] Here, "average particle size (D50)" refers to the median particle size (D50) measured by a laser diffraction / scattering particle size distribution measuring device. It should be noted that if the coating liquid used for the surface protective layer contains particles, the surface protective layer 5 obtained from that coating liquid also contains particles. The average particle size of the particles contained in the surface protective layer 5 can be obtained by observing its cross-section, measuring the particle size of multiple particles, and averaging the results. This value is substantially the same as the median particle size (D50) measured by the laser diffraction / scattering particle size distribution measuring device. Therefore, the aforementioned range of average particle size can also be read as the range of average particle size of the particles contained in the surface protective layer 5.

[0079] The particles are included in the surface protective layer 5 in an amount of 3 to 11 parts by mass relative to 100 parts by mass of resin. The amount of particles added is preferably 4 to 10 parts by mass relative to 100 parts by mass of resin. It should be noted that "100 parts by mass of resin" refers to the mass of the solid components of the resin.

[0080] When the particle addition amount is within the above range, the effect of uniform wrinkling is particularly significant. When the particle addition amount is high, a tendency to decrease the value of Rdc / t can be observed. Therefore, when the particle addition amount is too low or too high, it is difficult to achieve a "wet touch". In addition, when the particle addition amount is high, the particles are sometimes prone to detaching from the surface protective layer 5, making it difficult to achieve high scratch resistance. When the particle addition amount is low, the effect of uniform wrinkling is small.

[0081] The gloss of the surface protective layer 5 is less than 10.0. Preferably, the gloss of the surface protective layer 5 is 5 or less. Here, "gloss" is the measured value when measured with a gloss meter at an incident angle of 60 degrees according to JIS Z8741:1997.

[0082] <2> Manufacturing method of decorative sheet

[0083] Decorative sheet 1 is manufactured, for example, by the following method. Here, for the sake of simplicity, the description of pattern layer 3, transparent resin layer 4, primer layer 6, adhesive layer 7, and concealing layer 8 is omitted.

[0084] First, a coating film consisting of a surface protective layer coating liquid is formed on one surface of the raw material layer 2. This coating film can be formed by various printing methods such as gravure printing, offset printing, screen printing, electrostatic printing, inkjet printing, etc.; or by various coating methods such as roller coating, doctor blade coating, micro-gravure coating, mold coating, etc.

[0085] The coating liquid for the surface protective layer contains the aforementioned resin and particles. The coating liquid for the surface protective layer may also contain solvents or additives (e.g., antibacterial agents and antifungal agents) to improve the functionality of the final product. The coating liquid for the surface protective layer may also contain other additives such as ultraviolet absorbers and light stabilizers. Examples of ultraviolet absorbers include benzotriazole, benzoate, benzophenone, and triazine compounds. Examples of light stabilizers include hindered amine compounds. It should be noted that, according to the method described herein, a surface protective layer 5 with low gloss can be formed without a gloss modifier (matte additive).

[0086] In the second irradiation step described later, when the coating film composed of the surface protective layer coating liquid is cured as a whole by ultraviolet irradiation, the surface protective layer coating liquid preferably also contains a photoinitiator. There are no particular limitations on the photoinitiator; examples include benzophenone-based, acetophenone-based, benzoin ether-based, and thioxanthone-based photoinitiators.

[0087] After forming a coating film composed of a surface protective layer coating liquid, a first irradiation step is performed. In the first irradiation step, light with a wavelength of 200 nm or less (hereinafter referred to as first radiation) is irradiated onto the coating film. The ionizing radiation-curing resin contained in the surface protective layer coating liquid has a high absorption coefficient for the first radiation. Therefore, the first radiation incident on the coating film can only reach a position tens to hundreds of nm away from its outermost surface. Therefore, in the first irradiation step, a cross-linking reaction occurs in the surface area of ​​the coating film to form an extremely thin cured film, while in other areas, no cross-linking reaction occurs and the film remains uncured.

[0088] The coating after the first irradiation process has wrinkles on its surface corresponding to the ridge 5B. The inventors believe that the wrinkles are generated on the coating surface by the first irradiation process as follows.

[0089] As described above, the first radiation can only reach locations tens to hundreds of nm away from the outermost surface of the coating. That is, the cross-linking reaction of the ionizing radiation-curable resin occurs only on the surface of the coating, while regions further inward than tens to hundreds of nm from the outermost surface remain uncured, containing highly fluid molecules. These highly fluid molecules increase the volume of the cured film by causing it to swell. Relative to the in-plane compressive stress generated by this increase in volume, the cured film buckles, thereby creating wrinkles on the coating surface.

[0090] The first type of radiation can be extracted from excimer VUV (Vacuum Ultra Violet) light. Excimer VUV light can be generated by lamps using rare gases or rare gas halides. When high-energy electrons are applied from the outside to a lamp enclosed in a rare gas or rare gas halide gas, a large amount of discharge plasma (dielectric barrier discharge) is generated. Through this plasma discharge, the atoms of the discharge gas (rare gas) are excited and momentarily enter the excimer state. When returning from this excimer state to the ground state, light in the wavelength region specific to that excimer is emitted.

[0091] The gas used in excimer lamps only needs to emit light below 200 nm, and can be any gas previously used. As the gas, rare gases such as Xe, Ar, and Kr, as well as mixtures of rare gases and halogen gases such as ArBr and ArF, can be used. The wavelength (center wavelength) of the excimer lamp varies depending on the gas, for example, it has wavelengths of approximately 172 nm (Xe), approximately 126 nm (Ar), approximately 146 nm (Kr), approximately 165 nm (ArBr), and approximately 193 nm (ArF).

[0092] Considering the difference between the photon energy, wavelength, and binding energy of organic matter, a xenon lamp emitting excimer light with a center wavelength of 172 nm is preferred as the light source. Furthermore, if the cost of equipment maintenance and the availability of materials are also taken into account, a xenon lamp is also preferred as the light source.

[0093] The first irradiation step is carried out in an atmosphere with low oxygen concentration. Oxygen has a high absorption coefficient for light below 200 nm. Therefore, the first irradiation step is preferably carried out in a nitrogen atmosphere, for example. The oxygen concentration in the gas phase of the first irradiation step, i.e., the residual oxygen concentration in the reaction atmosphere, is preferably set to 2000 ppm or less, more preferably 1000 ppm or less.

[0094] Furthermore, oxygen in the atmosphere inhibits free radical polymerization. Therefore, the residual oxygen concentration in the reaction atmosphere affects the formation of wrinkles on the coating surface. Consequently, the surface properties of the surface protective layer 5 may also change when the residual oxygen concentration in the reaction atmosphere changes.

[0095] The cumulative intensity of the first radiation is preferably set to 0.5 mJ / cm². 2 Above 200mJ / cm 2 The following, and more preferably, is set to 1 mJ / cm 2 Above 100mJ / cm 2 The following is a further preferred setting: 3mJ / cm 2 Above 50mJ / cm 2 The optimal value is set to 5 mJ / cm. 2 Above 30mJ / cm 2 The following applies: When the cumulative light intensity is reduced, the in-plane expansion of the cured film decreases. When the cumulative light intensity is increased, the surface condition of the coating deteriorates.

[0096] After the first irradiation step is completed, the second irradiation step is performed. In the second irradiation step, the coating is cured by irradiating it with a second type of radiation. Thus, a surface protective layer 5 is obtained.

[0097] The second radiation is either ionizing radiation such as an electron beam, or ultraviolet radiation with a wavelength longer than the first radiation. When ultraviolet radiation is used as the second radiation, it has a wavelength at which the ionizing radiation-curing resin exhibits a smaller absorption coefficient.

[0098] The cumulative light intensity of the second radiation is preferably set to 10 mJ / cm². 2 Above 500mJ / cm 2 The following, and more preferably, setting it to 50 mJ / cm 2 Above 400mJ / cm 2 The following is a further preferred setting: 100 mJ / cm 2 Above 300mJ / cm 2the following.

[0099] Decorative sheet 1 can be manufactured, for example, by the methods described above. Decorative sheet 1 can also be manufactured by other methods. For example, for surface protective layer 5, a plate can be formed using the methods described above, and a transfer can be performed using the plate to form a surface protective layer 5 with an uneven structure on the surface.

[0100] <3> Effect

[0101] Reference Figures 1 to 3 The decorative sheet 1 described herein has a surface protective layer 5 with the aforementioned surface properties. When a user presses the surface of the protective layer 5 with their skin while simultaneously sliding their fingers across the surface, for example, when pressing the surface of the protective layer 5 with their fingers while sliding their fingers across the surface, the decorative sheet 1 provides a moist tactile sensation. That is, because the slope of the uneven surface of the protective layer 5 is relatively gentle, the pressure resistance caused by the contact between the fingers and the surface is minimized during the aforementioned touching action, and the contact area between the fingers and the raised surface gradually increases. Thus, a tactile sensation of the decorative sheet adhering to the fingers can be obtained.

[0102] The moist feel allows the person touching the decorative piece 1 to experience comfort and warmth. Furthermore, the moist feel lends the decorative piece 1 a sense of luxury. Therefore, the decorative piece 1, which provides a moist feel to the user, is suitable for applications where there is frequent or prolonged contact with the user's skin, such as tabletops, chair armrests, and railings for stairs or passageways.

[0103] Because the surface protective layer 5 of the decorative piece 1 has the aforementioned surface properties, a low gloss level can be achieved even without gloss modifiers (matte additives). Gloss modifiers reduce the oleophobicity of the layer formed from the resin material, thus the surface protective layer 5 containing gloss modifiers is prone to fingerprint adhesion. The surface protective layer 5 without gloss modifiers is less likely to absorb oil, thus fingerprints are less likely to adhere. In addition, the surface protective layer 5 with excellent oleophobicity is less likely to absorb oil or contaminants. Furthermore, when the surface of the surface protective layer 5 without gloss modifiers is scratched, the particles of the gloss modifier will not fall off, therefore, the decorative piece 1 including such a surface protective layer 5 is less prone to gloss changes and scratches.

[0104] The surface protective layer 5 with the above-mentioned surface properties can be obtained by the above method for the following reasons.

[0105] Oxygen in the gas phase not only absorbs short-wavelength ultraviolet light but also hinders free radical polymerization. The effect of oxygen in the gas phase on free radical polymerization is greatest in the portion of the coating film composed of ionizing radiation-curable resin adjacent to the gas phase, and decreases with increasing distance from the coating surface. Therefore, in the first irradiation step, by changing the oxygen concentration in the gas phase, the relationship between the distance from the coating surface and the degree of crosslinking reaction can be altered.

[0106] When this relationship changes, the thickness of the cured film produced on the surface of the coating through the first irradiation process and the degree of in-plane expansion of the cured film based on the cross-linking reaction change. The cumulative light intensity of the first irradiation process also affects the thickness of the cured film and the degree of in-plane expansion. Furthermore, the thickness of the cured film and the degree of in-plane expansion affect the surface properties of the surface protective layer. In addition, the particle size and amount of particles in the coating, as well as the thickness of the coating, also affect the formation of wrinkles.

[0107] Therefore, by appropriately setting the composition of the ionizing radiation curable resin, the particle size and amount of particles added, the thickness of the coating, the oxygen concentration in the gas phase of the first irradiation step, and the cumulative light intensity of the first irradiation step, a surface protective layer with desired surface properties can be obtained.

[0108] Example

[0109] Examples of the present invention are described below.

[0110] <Example 1>

[0111] The reference was created using the following method. Figures 1 to 3 Decorative piece 1 is shown in the illustration. It should be noted that, in this example, the transparent resin layer 4, primer layer 6, adhesive layer 7, and concealing layer 8 are omitted.

[0112] First, prepare a unit area mass of 50g / m². 2 Impregnated paper (GFR-506: manufactured by Kojin Co., Ltd.) is used as the base material layer 2. Using oil-based nitrocellulose resin gravure printing ink (PCNT (PCRNT) various colors: manufactured by Toyo Ink Co., Ltd.), a pattern layer 3 is formed on one side of the base material layer 2.

[0113] Next, a surface protective layer coating liquid is applied to the pattern layer 3. The surface protective layer coating liquid is a coating liquid formulated with the following particles in a ionizing radiation curable resin.

[0114] • Ionizing radiation-cured resin

[0115] Type: Trimethylolpropane EO-modified triacrylate (EO 15 molar addition)

[0116] Product Name: SR9035 (Made by Sartomer)

[0117] Mixture: 100 parts by weight

[0118] ·particle

[0119] Product Name: SYLYSIA 250N (Manufactured by Fuji Silysia Chemical Ltd.)

[0120] Particle size: 5μm

[0121] Mixture: 5 parts by weight

[0122] A coating film consisting of a surface protective layer and a coating liquid is formed in such a way that the thickness is 5 μm.

[0123] Then, the first irradiation step is performed. Specifically, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 500 ppm to achieve a cumulative light intensity of 50 mJ / cm². 2 The surface of a coating film consisting of a surface protective layer made of a coating liquid is irradiated with ultraviolet light with a wavelength of 172 nm. This causes wrinkles to form on the surface of the coating film.

[0124] Next, the second irradiation process is carried out. Specifically, the coating is cured by irradiating it with ionizing radiation, thereby forming a surface protective layer 5.

[0125] Decorative piece 1 was obtained through the above process.

[0126] <Comparative Example 1>

[0127] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, no particles were used.

[0128] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0129] <Comparative Example 2>

[0130] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 2 parts by mass.

[0131] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 90 mJ / cm². 2The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0132] <Example 2>

[0133] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 3 parts by mass.

[0134] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 250 ppm to achieve a cumulative light intensity of 70 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0135] <Example 3>

[0136] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 4 parts by mass.

[0137] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 400 ppm to achieve a cumulative light intensity of 60 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0138] <Example 4>

[0139] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 10 parts by mass.

[0140] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 750 ppm to achieve a cumulative light intensity of 40 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0141] <Example 5>

[0142] Except for the following aspects, decorative sheet 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 11 parts by mass.

[0143] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 750 ppm to achieve a cumulative light intensity of 40 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0144] <Comparative Example 3>

[0145] Except for the following aspects, decorative sheet 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 12 parts by mass.

[0146] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 750 ppm to achieve a cumulative light intensity of 40 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0147] <Comparative Example 4>

[0148] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, a coating film consisting of a surface protective layer made of a coating liquid was formed in such a way that the thickness was 1 μm.

[0149] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0150] <Example 6>

[0151] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, a coating film consisting of a surface protective layer made of a coating liquid was formed in such a way that the thickness was 2 μm.

[0152] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 80 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0153] <Example 7>

[0154] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, a coating film consisting of a surface protective layer made of a coating liquid was formed in such a way that the thickness was 3 μm.

[0155] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 200 ppm to achieve a cumulative light intensity of 70 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0156] <Example 8>

[0157] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, a coating film consisting of a surface protective layer coating liquid was formed in such a way that the thickness was 10 μm.

[0158] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 700 ppm to achieve a cumulative light intensity of 20 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0159] <Example 9>

[0160] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, a coating film consisting of a surface protective layer made of a coating liquid was formed in such a way that the thickness was 18 μm.

[0161] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 700 ppm to achieve a cumulative light intensity of 10 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0162] <Comparative Example 5>

[0163] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, a coating film consisting of a surface protective layer made of a coating liquid was formed in such a way that the thickness was 20 μm.

[0164] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 700 ppm to achieve a cumulative light intensity of 5 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0165] <Comparative Example 6>

[0166] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0167] ·particle

[0168] Product Name: SYLYSIA 310P (Manufactured by Fuji Silysia Chemical, Ltd.)

[0169] Particle size: 2μm

[0170] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 600 ppm to achieve a cumulative light intensity of 40 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0171] <Example 10>

[0172] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0173] ·particle

[0174] Product Name: SYLYSIA 420 (Manufactured by Fuji Silysia Chemical, Ltd.)

[0175] Particle size: 3μm

[0176] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 550 ppm to achieve a cumulative light intensity of 45 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0177] <Example 11>

[0178] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0179] ·particle

[0180] Product Name: SYLYSIA 430 (Manufactured by Fuji Silysia Chemical, Ltd.)

[0181] Particle size: 4μm

[0182] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 550 ppm to achieve a cumulative light intensity of 45 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0183] <Example 12>

[0184] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0185] ·particle

[0186] Product Name: SYLYSIA 450 (Manufactured by Fuji Silysia Chemical, Ltd.)

[0187] Particle size: 8μm

[0188] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 400 ppm to achieve a cumulative light intensity of 80 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0189] <Example 13>

[0190] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0191] ·particle

[0192] Product Name: SYLYSIA 882 (manufactured by Fuji Silysia Chemical, Ltd.)

[0193] Particle size: 10μm

[0194] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0195] <Example 14>

[0196] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0197] ·particle

[0198] Product Name: SYLYSIA 780 (Manufactured by Fuji Silysia Chemical, Ltd.)

[0199] Particle size: 11μm

[0200] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0201] <Example 15>

[0202] Except for the following aspects, decorative piece 1 was manufactured using the same method as in Example 1. That is, in this example, the following particles were used.

[0203] ·particle

[0204] Product Name: Sicastar 43-00-154 (Manufactured by CoreFront Corporation)

[0205] Particle size: 14μm

[0206] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0207] <Comparative Example 7>

[0208] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0209] • Ionizing radiation-cured resin

[0210] Type: Trimethylolpropane triacrylate

[0211] Product Name: NK ESTER A-TMPT (Made by Shin-Nakamura Chemical Co., Ltd.)

[0212] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0213] <Example 16>

[0214] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0215] • Ionizing radiation-cured resin

[0216] Type: Trimethylolpropane EO-modified triacrylate (EO3 molar addition)

[0217] Product Name: Miramer M3130 (Made by Miwon)

[0218] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0219] <Example 17>

[0220] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0221] • Ionizing radiation-cured resin

[0222] Type: Trimethylolpropane EO-modified triacrylate (EO6 molar addition)

[0223] Product Name: Miramer M3160 (Made by Miwon)

[0224] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0225] <Example 18>

[0226] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0227] • Ionizing radiation-cured resin

[0228] Type: Trimethylolpropane EO-modified triacrylate (EO9 molar addition)

[0229] Product Name: SR502 (Manufactured by Sartomer Company)

[0230] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 200 ppm to achieve a cumulative light intensity of 80 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0231] <Example 19>

[0232] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0233] • Ionizing radiation-cured resin

[0234] Type: Trimethylolpropane EO-modified triacrylate (EO20 molar addition)

[0235] Product Name: NK ESTER AT-20E (Manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0236] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 600 ppm to achieve a cumulative light intensity of 45 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0237] <Example 20>

[0238] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0239] • Ionizing radiation-cured resin

[0240] Type: Ethoxylated pentaerythritol tetraacrylate (EO20 molar addition)

[0241] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 600 ppm to achieve a cumulative light intensity of 45 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0242] <Example 21>

[0243] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0244] • Ionizing radiation-cured resin

[0245] Type: Ethoxylated pentaerythritol tetraacrylate (EO35 molar addition)

[0246] Product Name: NK ESTER ATM-35E (Manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0247] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 650 ppm to achieve a cumulative light intensity of 40 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0248] <Comparative Example 8>

[0249] Except for the following aspects, decorative sheet 1 was manufactured using the same method as in Example 1. That is, in this example, the amount of particles was set to 15 parts by mass.

[0250] Furthermore, the coating film composed of the surface protective layer coating liquid is cured only through the second irradiation process, without performing the first irradiation process.

[0251] <Comparative Example 9>

[0252] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0253] • Ionizing radiation-cured resin

[0254] Type: Ethylene glycol diacrylate (EO9 molar addition)

[0255] Product Name: Light Acrylate 9EG-A (Made by Kyoei Chemical Co., Ltd.)

[0256] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 550 ppm to achieve a cumulative light intensity of 40 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0257] <Comparative Example 10>

[0258] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0259] • Ionizing radiation-cured resin

[0260] Type: Ethoxylated pentaerythritol hexaacrylate (EO12 molar addition)

[0261] Product Name: NK ESTER A-DPH-12E (Manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0262] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0263] <Comparative Example 11>

[0264] Except for the following aspects, the decorative sheet 1 was manufactured by the same method as in Example 1. That is, in this example, the following ionizing radiation-curable resin was used.

[0265] • Ionizing radiation-cured resin

[0266] Type: Pentaerythritol tetraacrylate

[0267] Product Name: NK ESTER A-TMMT (Made by Shin-Nakamura Chemical Co., Ltd.)

[0268] Furthermore, in the first irradiation process, an Xe excimer lamp is used in a nitrogen atmosphere with atmospheric pressure and an oxygen concentration of 100 ppm to achieve a cumulative light intensity of 100 mJ / cm². 2 The surface of the coating film, which is composed of a surface protective layer and a coating liquid, is irradiated with ultraviolet light with a wavelength of 172 nm.

[0269] <Evaluation>

[0270] The following evaluation is made of each of the above decorative pieces.

[0271] (1) Thickness of surface protective layer

[0272] The thickness of the surface protective layer was measured as follows. Decorative sheet 1 was embedded in a cold-curing epoxy resin or UV-curing resin and allowed to fully cure. It was then cut to reveal its cross-section, and mechanically ground to obtain the measurement surface. Next, the thickness of the surface protective layer was measured using a SIGMA 500 scanning electron microscope manufactured by Carl Zeiss Microscopy GmbH. Measurements were taken at any 25 points, and the average of these 25 measurements was defined as the "thickness t of the surface protective layer". The measurement conditions were set as follows: accelerating voltage of 0.5 keV (low accelerating voltage), imaging mode SE2, and magnification of 2000x. The sample was not sputtered. The "thickness t of the surface protective layer" is equal to the thickness of the coating film formed by the surface protective layer coating liquid.

[0273] (2) Gloss

[0274] Gloss was measured at 60 degrees using a Rhopoint IQ (manufactured by Konica Minolta, Inc.). The "60-degree gloss value" in Tables 1 to 4 below represents this 60-degree gloss.

[0275] (3) Skin feel

[0276] The following methods can be used to evaluate skin feel.

[0277] First, preparations were made to ensure consistency in evaluation criteria among evaluators. Specifically, three standard test pieces with different surface properties were prepared. Next, five evaluators, blindfolded, pressed their fingers against the surface of the standard test pieces while sliding their fingers across the surface, and then categorized the tactile sensations into the following three groups.

[0278] Group 1: There is almost no resistance to pressing in, but you can feel the surface of the decorative piece adhering to your fingers, and you can also get a smooth gliding feel. Overall, the impression of a smooth gliding feel is enhanced. That is, you get a smooth feel.

[0279] Group 2: There is almost no resistance to pressing in, but you can feel the surface of the decorative piece adhering to your fingers. However, there is no impression of a smooth, gliding feel. In other words, you get a wet feel.

[0280] Group 3: You feel resistance when pressing in, and at the same time, you feel the presence of unevenness. That is, you get a rough tactile sensation.

[0281] Repeat the above steps until all evaluators' evaluations are consistent for three consecutive times, and the evaluation results among the evaluators are consistent for three consecutive times.

[0282] Next, for each of the aforementioned decorative pieces, the evaluators, while blindfolded, pressed their fingers against the surface of the protective layer while simultaneously sliding their fingers across the surface. The tactile sensation was then categorized into the three groups mentioned above. This process was repeated until each evaluator's evaluation was consistent for at least three consecutive times, and the evaluation results among the evaluators were also consistent for three consecutive times. Based on this result, the skin feel was evaluated according to the following criteria.

[0283] A (Smooth): Group 1

[0284] B (Moist): Group 2

[0285] C (Rough): Group 3

[0286] (4) Fingerprint resistance

[0287] As a fingerprint resistance evaluation, a fingerprint wiping resistance evaluation was conducted.

[0288] Specifically, firstly, the 60-degree gloss of each decorative piece's surface was measured, and this 60-degree gloss was taken as the initial gloss. Next, a fingerprint resistance evaluation solution was applied to the surface protective layer, and the fingerprint resistance evaluation solution applied to the decorative piece's surface was wiped off. Here, a higher fatty acid was used as the fingerprint resistance evaluation solution. Then, the 60-degree gloss of the portion after wiping off the fingerprint resistance evaluation solution was measured, and this 60-degree gloss was taken as the post-wiping gloss.

[0289] The fingerprint wiping rate is calculated according to the following formula.

[0290] Fingerprint wiping rate (%) = (gloss after wiping / initial gloss) × 100

[0291] The evaluation criteria are as follows.

[0292] AA: 70% or more but less than 250%

[0293] A: 50% or more but less than 70%, or 250% or more but less than 300%.

[0294] B: Less than 50%, or more than 300%

[0295] (5) Stain resistance

[0296] As an evaluation of stain resistance, the Stain A test as specified in the Japanese Agricultural Standards (JAS) was conducted. Specifically, 10mm wide lines were drawn on the protective layer of each decorative piece using blue ink, black quick-drying ink, and red crayon, respectively, and left for 4 hours. Then, the lines using the blue ink, black quick-drying ink, and red crayon were wiped with a cloth containing ethanol.

[0297] The evaluation criteria are as follows.

[0298] AA: It can easily wipe off threads of various colors.

[0299] A: You can wipe part of the lines of each color, but some will still have dirt left.

[0300] B: Do not wipe the lines of different colors.

[0301] (6) Damage resistance

[0302] Each decorative panel was adhered to the wood substrate B using a urethane-based adhesive. Then, a stainless steel wool abrasion test was performed as an evaluation of scratch resistance. Specifically, the decorative panel was rubbed back and forth with stainless steel wool 20 times while a load of 100g was applied, and the damage and gloss changes on the surface of the decorative panel were visually confirmed.

[0303] The evaluation criteria are as follows.

[0304] AA: No surface damage or change in gloss.

[0305] A: The surface has suffered minor damage or a change in gloss.

[0306] B: The surface has obvious damage or changes in gloss.

[0307] (7) Processability

[0308] The obtained decorative sheet is adhered to the wood substrate B with the original material layer side (i.e., the back of the decorative sheet) facing the wood substrate B using a urethane adhesive. Then, the V-groove is inserted into the boundary between the wood substrate B and the decorative sheet without damaging the decorative sheet.

[0309] Next, the wood substrate B was bent along the V-groove to 90 degrees, causing the surface of the decorative sheet (i.e., the surface of the decorative sheet) to become folded. The bending workability was evaluated by observing the bent portion of the decorative sheet surface for whitening or cracking using an optical microscope.

[0310] The evaluation criteria are as follows.

[0311] AA: No whitening or cracking was observed.

[0312] A: Some observations show whitening.

[0313] B: Whitening is observed on the entire surface, or cracking is observed on a portion of the surface.

[0314] (8) Cross-sectional height difference Rdc and ratio Rdc / t

[0315] The cross-sectional height difference Rdc (μm) and the ratio Rdc / t are calculated as detailed above.

[0316] The evaluation results are shown in Tables 1 to 4. In Tables 1 to 4, when the skin feel evaluation result is A (smooth), it is indicated by writing the character Y in the "A (smooth)" column; when the skin feel evaluation result is B (moist), it is indicated by writing the character Y in the "B (moist)" column; and when the skin feel evaluation result is C (rough), it is indicated by writing the character Y in the "C (rough)" column.

[0317] [Table 1]

[0318]

[0319] [Table 2]

[0320]

[0321] [Table 3]

[0322]

[0323] [Table 4]

[0324]

[0325] As shown in Tables 1 to 4, the decorative sheets described in Examples 1 to 21 impart a moist tactile feel to the evaluator. Furthermore, the decorative sheets described in Examples 1 to 21 exhibit low gloss and excellent fingerprint resistance, stain resistance, and processability. In addition, the decorative sheets described in Examples 1 to 14 and 16 to 21 also demonstrate excellent scratch resistance.

[0326] As shown in Table 1, Comparative Example 3 imparted a moist feel to the evaluators and had a low gloss, but its resistance to stains, scratches, and processability was poor. As shown in Table 4, Comparative Example 8 imparted a moist feel to the evaluators, but had a high gloss and poor resistance to fingerprints, stains, and scratches.

[0327] In contrast, as shown in Tables 1, 2, and 4, Comparative Examples 1, 2, 5, 6, and 9 did not provide the evaluators with a moist feel, but rather a rough feel. Furthermore, as shown in Tables 2 to 4, Comparative Examples 4, 7, 10, and 11 did not provide the evaluators with a moist feel, but rather a smooth feel.

[0328] Explanation of symbols

[0329] 1…Decorative sheet, 2…Material layer, 3…Pattern layer, 4…Transparent resin layer, 5…Surface protective layer, 6…Primer layer, 7…Adhesive layer, 8…Hidden layer, 11…Decorative material, B…Substrate.

Claims

1. A decorative sheet comprising a base material layer and a surface protective layer disposed on one surface of the base material layer, The surface of the protective layer is provided with a concave-convex structure comprising multiple ridge-shaped portions, each protruding in a ridge-like manner. The ratio of the cross-sectional height difference Rdc of the uneven structure of the surface protective layer to the thickness t of the surface protective layer, Rdc / t, is greater than 0.1 and less than 0.

2. The thickness t of the surface protective layer is more than 5 μm and less than 18 μm. The surface protective layer contains cured resin products and particles, wherein the average particle size is 3 μm to 11 μm, and the particles are contained in the surface protective layer in an amount of 3 to 11 parts by mass relative to 100 parts by mass of the resin. The gloss level of the surface protective layer is less than 10. The resin is a trifunctional acrylate containing repeating structures, wherein the repeating structure has 3 to 20 repeatings, or The resin is a tetrafunctional acrylate containing repeating structures, wherein the repeating structure has 20 to 35 repeatings. The repeating structure is any one of the following: ethylene oxide structure, propylene oxide structure, and ε-caprolactone structure. The cross-sectional height difference Rdc is a surface property parameter specified in JIS B0601:2013. The highest peak position of the roughness curve is set as the reference for the cross-sectional height c. c(Rmr1) is set as the cross-sectional height when the load length ratio Rmr of the roughness curve is 10%, and c(Rmr2) is set as the cross-sectional height when the load length ratio Rmr of the roughness curve is 25%. The cross-sectional height difference Rdc is the difference between the cross-sectional heights c(Rmr1) and c(Rmr2), wherein the unit of the cross-sectional height difference Rdc is μm. The average particle size is the median particle size D50 obtained by laser diffraction / scattering particle size distribution measurement device; or it is the value obtained by observing the cross-section of the surface protective layer, measuring the particle size of multiple particles, and averaging them. The gloss level is the measured value obtained using a gloss meter at an incident angle of 60 degrees, according to JIS Z8741:1997.

2. The decorative piece according to claim 1, wherein, A patterned layer is also provided between the raw material layer and the surface protective layer.

3. A decorative material, comprising: The decorative piece as described in claim 1 or 2, and The substrate for attaching the decorative piece.

Citation Information

Patent Citations

  • Decorative material

    JP2019119138A

  • Decorative sheet

    JP2021165033A