A method for treating alkyd resin esterification wastewater and its application
Alkyd resin paint is prepared by reacting calcium oxide and carbon dioxide to generate an intermediate, which is then combined with alkyd resin and additives. This solves the problem of high COD value in alkyd resin esterification wastewater, and realizes low-carbon and environmentally friendly resource utilization and improved economic benefits.
Patent Information
- Application Number
- CN202411410576.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-10-10
AI Technical Summary
The high COD value of alkyd resin esterification wastewater leads to high treatment costs and a lack of low-carbon and environmentally friendly resource utilization methods.
Alkyd resin paint is prepared by reacting calcium oxide and carbon dioxide to generate an intermediate, which is then combined with alkyd resin and additives. Modified polyvinyl alcohol is used to improve reaction efficiency and activity, reduce calcium oxide residue, and generate raw materials that can be used in alkyd resin paint.
It reduces the cost of esterification wastewater treatment, achieves low-carbon and environmentally friendly utilization of resources, reduces pollution, and improves economic benefits.
Smart Images

Figure BDA0005077871740000081
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating technology, specifically relating to a method for treating alkyd resin esterification wastewater and its application. Background Technology
[0002] Alkyd resin esterification wastewater is generated during the polycondensation reaction between raw materials in the production of alkyd resin. The COD value of esterification wastewater is high, generally between 100,000 and 200,000 kilovolts, and cannot be directly discharged. It must be safely treated by a professional wastewater treatment company, with treatment costs of approximately 3,000 to 4,000 yuan per ton. As of 2023, the annual production of alkyd resin was approximately 2.6 million tons. Based on the calculation that each ton of alkyd resin generates 30 kilograms of wastewater, approximately 78,000 tons of esterification wastewater are generated annually, with treatment costs for professional companies amounting to approximately 234 million yuan per year.
[0003] Therefore, there is an urgent need to develop a treatment method for alkyd resin esterification wastewater to address the current lack of low-carbon and environmentally friendly resource utilization methods for alkyd resin esterification wastewater. Summary of the Invention
[0004] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the present invention proposes a method for treating alkyd resin esterification wastewater. Through a secondary reaction, the esterification wastewater is transformed into a raw material that can be used in alkyd resin paints, reducing pollution, lowering costs, and improving economic benefits.
[0005] According to a first aspect of the present invention, a method for treating alkyd resin esterification wastewater is provided, comprising the following steps:
[0006] S1. Calcium oxide is added to alkyd resin esterification wastewater and heated to react, yielding intermediate A;
[0007] S2. Intermediate A is reacted with carbon dioxide to obtain intermediate B;
[0008] S3. Alkyd resin, additives and intermediate B are mixed and dispersed to prepare alkyd resin paint.
[0009] According to some embodiments of the present invention, the weight ratio of the alkyd resin esterification wastewater to the calcium oxide is 1:2.5 to 3.15.
[0010] Within the above range, excessive residues of alkyd resin esterification wastewater and calcium oxide were avoided, which could affect the second-step reaction.
[0011] According to some embodiments of the present invention, the weight ratio of the alkyd resin esterification wastewater to the calcium oxide is 1:2.85.
[0012] When the ratio of esterification wastewater to calcium oxide is 1:2.85, the degree of reaction is above 90%, which largely avoids the impact of excessive residues of alkyd resin esterification wastewater and calcium oxide on the second step of the reaction.
[0013] According to some embodiments of the present invention, the weight ratio of intermediate A to carbon dioxide is 1:0.5 to 0.75.
[0014] According to some embodiments of the present invention, the weight ratio of intermediate A to carbon dioxide is 1:0.65.
[0015] According to some embodiments of the present invention, step S1 further includes the addition of modified polyvinyl alcohol.
[0016] According to some embodiments of the present invention, the method for preparing the modified polyvinyl alcohol includes: dispersing polyvinyl alcohol, maleic anhydride and triethanolamine and reacting them at 70-100°C for 3-5 hours.
[0017] This invention utilizes the hydrogen bond formed between the hydroxyl groups of polyvinyl alcohol and the hydroxyl groups of calcium hydroxide in intermediate A. Subsequently, the hydroxyl groups on the surface of cellulose combine with the hydroxyl groups on the surface of partially unreacted calcium oxide, allowing calcium hydroxide to be fixed to the surface of undigested calcium oxide particles through cellulose, thus acting as a homogeneous seed crystal and providing a stable nucleus for calcium hydroxide crystallization. This makes it easier for calcium hydroxide molecules to aggregate and arrange around the nucleus, thereby accelerating the crystallization process. The increased crystallization rate means that more crystals are generated per unit time, which usually promotes crystal refinement and increases the specific surface area. The larger specific surface area provides more reaction sites, increasing the reaction rate of calcium hydroxide with carbon dioxide (CO2) and thus accelerating the formation of calcium carbonate. The modified polyvinyl alcohol contains carboxyl groups, and its addition makes the esterification wastewater slightly acidic, which helps reduce the binding of calcium and magnesium ions with the reactants, thereby improving the activity of the reactants.
[0018] According to some embodiments of the present invention, the additives include anti-settling agents, dispersants, pigments and fillers, driers and anti-skinning agents.
[0019] According to some embodiments of the present invention, the weight ratio of the anti-settling agent, the dispersant, the pigments and fillers, the intermediate B, the drier, and the anti-skinning agent is (0.3-1.5):(0.2-0.8):(20-30):(10-20):(0.5-1.5):(0.2-0.5).
[0020] According to some embodiments of the present invention, the additive further includes a solvent.
[0021] According to some embodiments of the present invention, the weight ratio of the alkyd resin, the solvent, the anti-settling agent, the dispersant, the pigments and fillers, the intermediate B, the drier and the anti-skinning agent is: (35-50): (7-18): (0.3-1.5): (0.2-0.8): (20-30): (10-20): (0.5-1.5): (0.2-0.5).
[0022] According to some embodiments of the present invention, the weight ratio of the alkyd resin, the solvent, the anti-settling agent, the dispersant, the pigments and fillers, the intermediate B, the drier, and the anti-skinning agent is 43:13:0.5:0.3:24:18:0.8:0.4.
[0023] According to some embodiments of the present invention, in step S1, the calcium oxide is added in batches to the alkyd resin esterification wastewater.
[0024] According to some embodiments of the present invention, the temperature of the heating reaction is 70–85°C.
[0025] According to some embodiments of the present invention, the step of mixing and dispersing alkyd resin, additives and intermediate B includes: mixing and dispersing alkyd resin, anti-settling agent and dispersant, then adding pigments and fillers and intermediate B and continuing to disperse, then adding drier and anti-skinning agent.
[0026] According to some embodiments of the present invention, the step of mixing and dispersing alkyd resin, additives and intermediate B includes: adding solvent, anti-settling agent and dispersant sequentially to alkyd resin under stirring at 400-600 rpm, and then dispersing at 800-1000 rpm for 10-15 minutes; then adding pigments and fillers and intermediate B and continuing to disperse at 800-1000 rpm for 15-30 minutes, grinding through a sand mill to a fineness of <40 micrometers, and finally adding driers and anti-skinning agents, and dispersing at 600-800 rpm for 10-15 minutes to obtain alkyd resin paint.
[0027] According to a second aspect of the present invention, an alkyd resin paint is provided, which is prepared by the aforementioned method for treating alkyd resin esterification wastewater.
[0028] According to a third aspect of the present invention, an alkyd resin paint is proposed for use in steel structure workshops, bridges, and mechanical equipment. Detailed Implementation
[0029] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.
[0030] Alkyd resins are air-drying alkyd resins, specifically: Sanmu Chemical, D&S Tongde AK2970X, AK2965;
[0031] The solvents are aromatic hydrocarbon solvents, specifically toluene, xylene, and trimethylbenzene.
[0032] Ester solvents specifically include: butyl acetate, dimethyl carbonate, and ethyl acetate.
[0033] Anti-settling agents include bentonite, specifically: Hemings SD-1, SD-2, Walter BP-183B, or Fenghong BS-1C.
[0034] Dispersants include organosiloxane polymers, specifically BYK-P104S or TEGO-270.
[0035] The pigments and fillers specifically include: barium sulfate, talc, titanium dioxide, phthalocyanine blue, ultramarine, lemon yellow, or carbon black.
[0036] The drying agent is specifically one of the following: cobalt isooctanoate, manganese isooctanoate, or zinc isooctanoate.
[0037] The anti-skinning agent is specifically methyl ethyl ketone oxime or 2,6-di-tert-butyl-p-cresol.
[0038] Example 1
[0039] A method for treating alkyd resin esterification wastewater, comprising the following preparation steps:
[0040] The wastewater from the esterification of acid resins contains, by mass ratio, 94.07% water, 1.9% ethylene glycol, 1.38% propylene glycol, 1.0% glycerol, 0.86% phthalic acid, and 0.59% benzoic acid.
[0041] S1. 100 parts of alkyd resin esterification wastewater were put into a reactor equipped with a heat collection device. 100 parts of calcium oxide were slowly added for the first time. When the temperature rose to 70°C, heat collection was started for use in the workshop heating room. After the reaction stabilized, 100 parts of calcium oxide were slowly added for the second time and heat collection was continued. Then, 85 parts of calcium oxide were slowly added for the third time and heat collection was continued to obtain the reaction product calcium hydroxide, which was labeled as intermediate A.
[0042] S2. While stirring, 250 parts of carbon dioxide are introduced into intermediate A to obtain the reaction product calcium carbonate. The dried and pulverized product is labeled as intermediate B.
[0043] S3. 43 parts of alkyd resin (Dearson Tongde AK2970X) were stirred at 450 rpm, and 13 parts of toluene, 0.5 parts of Walter BP-183B, and 0.3 parts of dispersant BYK-P104S were added sequentially. The mixture was then dispersed at 900 rpm for 12 minutes. Then, 24 parts of barium sulfate and 18 parts of intermediate B were added and the mixture was dispersed at 800 rpm for 20 minutes. The mixture was then ground in a sand mill until the fineness was <40 microns. Finally, 0.8 parts of drier cobalt isooctanoate and 0.4 parts of anti-skinning agent methyl ethyl ketone oxime were added and the mixture was dispersed at 700 rpm for 15 minutes to obtain the alkyd resin paint.
[0044] Example 2
[0045] A method for treating alkyd resin esterification wastewater, comprising the following preparation steps:
[0046] The wastewater from the esterification of acid resins contains, by mass ratio, 94.07% water, 1.9% ethylene glycol, 1.38% propylene glycol, 1.0% glycerol, 0.86% phthalic acid, and 0.59% benzoic acid.
[0047] S1. 100 parts of alkyd resin esterification wastewater were put into a reactor equipped with a heat collection device. 75 parts of calcium oxide were slowly added for the first time. When the temperature rose to 60°C, heat collection was started for use in the workshop heating room. After the reaction stabilized, 70 parts of calcium oxide were slowly added for the second time and heat collection was continued. Then, 75 parts of calcium oxide were slowly added for the third time and heat collection was continued. Then, 70 parts of calcium oxide were slowly added for the fourth time and heat collection was continued. The reaction product calcium hydroxide was obtained and labeled as intermediate A.
[0048] S2. While stirring, 265 parts of carbon dioxide were introduced into intermediate A to obtain the reaction product calcium carbonate. The dried and pulverized product was labeled as intermediate B.
[0049] S3. 45 parts of alkyd resin AK2965 were stirred at 500 rpm, and 11 parts of solvent butyl acetate, 0.6 parts of anti-settling agent Hemings SD-1, and 0.4 parts of dispersant Hemings SD-1 were added sequentially. The mixture was then dispersed at 850 rpm for 13 minutes. Then, 26 parts of pigments and fillers and 16 parts of intermediate B were added and the mixture was dispersed at 900 rpm for 25 minutes. The mixture was then ground in a sand mill until the fineness was <40 microns. Finally, 0.5 parts of drier cobalt isooctanoate and 0.3 parts of anti-skinning agent methyl ethyl ketone oxime were added and the mixture was dispersed at 750 rpm for 12 minutes to obtain the alkyd resin paint.
[0050] Example 3
[0051] A method for treating alkyd resin esterification wastewater, comprising the following preparation steps:
[0052] The wastewater from the esterification of acid resins contains, by mass ratio, 94.07% water, 1.9% ethylene glycol, 1.38% propylene glycol, 1.0% glycerol, 0.86% phthalic acid, and 0.59% benzoic acid.
[0053] S1. 100 parts of alkyd resin esterification wastewater were put into a reactor equipped with a heat collection device. 85 parts of calcium oxide were slowly added for the first time. When the temperature rose to 65°C, heat collection was started for use in the workshop heating room. After the reaction stabilized, 110 parts of calcium oxide were slowly added for the second time and heat collection continued. Then, 95 parts of calcium oxide were slowly added for the third time and heat collection continued. The reaction product calcium hydroxide was obtained and labeled as intermediate A.
[0054] S2. While stirring, 240 parts of carbon dioxide were introduced into intermediate A to obtain the reaction product calcium carbonate. The dried and pulverized product was labeled as intermediate B.
[0055] S3. While stirring 41 parts of alkyd resin at 600 rpm, add 14 parts of solvent toluene, 0.8 parts of anti-settling agent Hemings SD-1, and 0.6 parts of dispersant BYK-P104S sequentially, then disperse at 800 rpm for 15 minutes. Next, add 21 parts of pigment / filler talc powder and 20 parts of intermediate B, and continue dispersing at 750 rpm for 18 minutes. Grind the mixture through a sand mill until the fineness is <40 microns. Finally, add 0.9 parts of drying agent cobalt isooctanoate and 0.3 parts...
[0056] An anti-skinning agent was dispersed at 750 rpm for 11 minutes to prepare an alkyd resin paint.
[0057] Example 4
[0058] A method for treating alkyd resin esterification wastewater, comprising the following preparation steps:
[0059] The wastewater from the esterification of acid resins contains, by mass ratio, 94.07% water, 1.9% ethylene glycol, 1.38% propylene glycol, 1.0% glycerol, 0.86% phthalic acid, and 0.59% benzoic acid.
[0060] S1. 100 parts of alkyd resin esterification wastewater were put into a reactor equipped with a heat collection device. 100 parts of calcium oxide and 10 parts of modified polyvinyl alcohol were slowly added for the first time. When the temperature rose to 70°C, heat collection was started for use in the workshop heating room. After the reaction stabilized, 100 parts of calcium oxide were slowly added for the second time and heat collection continued. Then, 85 parts of calcium oxide were slowly added for the third time and heat collection continued. The reaction product calcium hydroxide was obtained and labeled as intermediate A.
[0061] S2. While stirring, 250 parts of carbon dioxide are introduced into intermediate A to obtain the reaction product calcium carbonate. The dried and pulverized product is labeled as intermediate B.
[0062] S3. 43 parts of alkyd resin AK2970X were stirred at 450 rpm, and 13 parts of solvent dimethyl carbonate, 0.5 parts of anti-settling agents SD-1 and SD-2, and 0.3 parts of dispersant BYK-P104S were added sequentially. The mixture was then dispersed at 900 rpm for 12 minutes. Then, 24 parts of pigment / filler talc powder and 18 parts of intermediate B were added and the mixture was dispersed at 800 rpm for 20 minutes. The mixture was then ground in a sand mill until the fineness was <40 microns. Finally, 0.8 parts of drier cobalt isooctanoate and 0.4 parts of anti-skinning agent methyl ethyl ketone oxime were added and the mixture was dispersed at 700 rpm for 15 minutes to obtain the alkyd resin paint.
[0063] The method for preparing the polyvinyl alcohol is as follows: 100 parts of polyvinyl alcohol, 10 parts of maleic anhydride and 5 parts of triethanolamine are dispersed in water and reacted at 70°C for 3 hours.
[0064] Comparative Example 1
[0065] The difference between this comparative example and Example 1 is that steps S1 and S2 are omitted, and intermediate B in step S3 is replaced with an equal amount of commercially available calcium carbonate.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 2 is that the esterification wastewater in step S1 is treated by a sewage treatment plant, and steps S2 and S3 are omitted.
[0068] Test Example 1
[0069] Product performance and cost comparison table:
[0070] In accordance with relevant national standards, product performance tests and economic data comparisons were conducted on Examples 1-3 and Comparative Examples 1-2, and the results are shown in Table 1.
[0071] Table 1 Performance Tests of Examples and Comparative Examples
[0072]
[0073] As shown in Table 1, the application scheme of the example can neutralize 240-305 kg of carbon dioxide per 100 kg of esterification wastewater, without additional esterification wastewater treatment costs, achieving low-carbon and environmentally friendly treatment. Since the raw materials are partially self-produced, the cost is reduced by approximately 0.5 yuan / kg compared to conventional alkyd resin paints. Furthermore, the reaction degree in Example 1 is above 90%, further minimizing the impact of excessive residual alkyd resin esterification wastewater and calcium oxide on the second-step reaction.
[0074] In Example 4, hydrogen bonds are formed between the hydroxyl groups of polyvinyl alcohol and the hydroxyl groups of calcium hydroxide in intermediate A. Subsequently, the hydroxyl groups on the surface of cellulose combine with the hydroxyl groups on the surface of partially unreacted calcium oxide. This allows calcium hydroxide to be fixed to the surface of undigested calcium oxide particles through cellulose, acting as a homogeneous seed crystal and providing a stable nucleus for calcium hydroxide crystallization. This makes it easier for calcium hydroxide molecules to aggregate and align around the nucleus, thus accelerating the crystallization process. The increased crystallization rate means more crystals are generated per unit time, which typically promotes crystal refinement and increases the specific surface area. A larger specific surface area provides more reaction sites, allowing for the neutralization of more carbon dioxide.
[0075] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.
Claims
1. A method for treating alkyd resin esterification wastewater, characterized in that, Includes the following steps: S1. Calcium oxide is added to alkyd resin esterification wastewater and heated to react, yielding calcium hydroxide; S2. Carbon dioxide is passed into calcium hydroxide to react and produce calcium carbonate. S3. Alkyd resin, additives and calcium carbonate are mixed and dispersed to prepare alkyd resin paint; The weight ratio of the alkyd resin esterification wastewater to the calcium oxide is 1:2.5~3.15; The weight ratio of calcium hydroxide to carbon dioxide is 1:0.5~0.75; Step S1 also includes adding modified polyvinyl alcohol, the preparation method of which includes dispersing polyvinyl alcohol, maleic anhydride and triethanolamine and reacting them at 70~100℃ for 3~5h.
2. The method for treating alkyd resin esterification wastewater according to claim 1, characterized in that, Additives include anti-settling agents, dispersants, pigments and fillers, driers, and anti-skinning agents.
3. The method for treating alkyd resin esterification wastewater according to claim 2, characterized in that, The weight ratio of the anti-settling agent, the dispersant, the pigments and fillers, the calcium carbonate, the drier, and the anti-skinning agent is (0.3~1.5):(0.2~0.8):(20~30):(10~20):(0.5~1.5):(0.2~0.5).
4. The method for treating alkyd resin esterification wastewater according to claim 1, characterized in that, In step S1, the calcium oxide is added to the alkyd resin esterification wastewater in batches.
5. The method for treating alkyd resin esterification wastewater according to claim 3, characterized in that, The step of mixing and dispersing the alkyd resin, additives and calcium carbonate includes: mixing and dispersing the alkyd resin, anti-settling agent and dispersant, then adding pigments, fillers and calcium carbonate and continuing to disperse, then adding a drier and an anti-skinning agent.
6. An alkyd resin paint, characterized in that, The alkyd resin paint is prepared by a method for treating alkyd resin esterification wastewater as described in any one of claims 1 to 5.
7. The application of the alkyd resin paint as described in claim 6 in steel structure workshops, bridges, and mechanical equipment.
Citation Information
Patent Citations
Process for treating waste water
JP1977079561A
Wastewater treatment method using carbonization technique
KR1019990014574A