A method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield
By preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield, the problems of low yield and instability of existing blue nanomaterials have been solved, and the high stability and high efficiency of the nanosheets have been achieved, expanding their application in optoelectronic devices and biomedicine.
Patent Information
- Application Number
- CN202411363200.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-09-27
AI Technical Summary
Existing blue light nanomaterials suffer from low fluorescence quantum yield, small size, and instability, failing to meet high-performance requirements and affecting the luminous efficiency and lifespan of optoelectronic devices.
A method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield was adopted. By preparing precursor solutions A and B, a nanosheet stock solution was synthesized. Then, through passivation of nanosheet surface defects and purification processes, blue nanosheets with high stability and high fluorescence quantum yield were obtained.
This improved the structural stability and fluorescence quantum yield of nanosheets, enhanced their resistance to external interference, enabled precise control of size and thickness, and improved the luminous efficiency and display quality of optoelectronic devices.
Smart Images

Figure CN119432376B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of nanomaterials and display lighting, specifically to a method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield. Background Technology
[0002] Blue light materials, as an indispensable key element in modern technology, play a crucial role in many cutting-edge fields. In the field of light-emitting diodes (LEDs), it is one of the core elements for achieving energy-efficient lighting and high-definition displays. In display technology, the clever combination of blue light with other colors can present vibrant, realistic, and clear full-color images, bringing people a stunning visual experience. In the field of bioimaging, blue light acts like a magical "probe," penetrating deep into cells to accurately image cellular structure and function, providing a powerful tool for disease diagnosis and medical research. In the field of photocatalysis, blue light plays a vital role in activating catalysts, promoting the efficient conduct of chemical reactions, and providing new avenues for solving energy and environmental problems.
[0003] However, existing blue light-emitting nanomaterials have several shortcomings in performance. Traditional blue light-emitting nanomaterials often have low fluorescence quantum yields, which acts like a funnel, causing a significant loss of energy during the luminescence process, resulting in a substantial reduction in luminous efficiency and failing to meet the growing demand for high performance. Simultaneously, their small size limits their application in optoelectronic devices; for example, in display screens, it may affect image clarity and brightness uniformity. Furthermore, poor stability is a pressing issue. These materials are easily affected by external environmental factors (such as changes in light intensity, temperature fluctuations, and humidity), leading to performance degradation, shortened lifespan, and increased operating costs.
[0004] In light of this, to meet the urgent needs of modern technology for high-performance optoelectronic devices and advanced biomedical applications, the development of a method for preparing blue nanosheets with high fluorescence quantum yield, ultra-large size, and good stability has become a focus of attention for both the scientific and industrial communities. The emergence of this novel material not only promises to significantly improve the luminous efficiency and display quality of optoelectronic devices, enabling them to stand out in a highly competitive market, but also provides more sensitive and accurate detection and diagnostic tools for research and clinical applications in the biomedical field, contributing to the development of human health. Summary of the Invention
[0005] This invention provides a method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield, the specific steps of which are as follows:
[0006] S1: Prepare precursor solution A;
[0007] S2: Prepare precursor solution B;
[0008] S3: The original solution for synthesizing nanosheets;
[0009] S4: Passivates surface defects on nanosheets;
[0010] S5: Purified perovskite blue light nanosheets.
[0011] Furthermore, step S1 specifically includes:
[0012] Salt A, organic ligand and non-coordination solvent are thoroughly mixed, heated to a certain temperature T1, and stirred for a predetermined time to successfully obtain a clear and transparent cesium precursor solution A.
[0013] Furthermore, step S2 specifically includes:
[0014] The lead halide and non-coordinate solvent are mixed, then vacuumed, and the mixed solution is raised to a certain temperature T2. Then, organic anionic ligands and organic cationic ligands are added, and the solution is raised to a certain temperature T3. The mixture is stirred for a certain time until the solution becomes clear and transparent, thus obtaining precursor solution B.
[0015] Furthermore, step S3 specifically includes:
[0016] Precursor solution B is heated to temperature T4 and stirred at a certain rate. Then, precursor solution A is injected into precursor solution B at a certain rate using a peristaltic pump. After reacting for a certain time, the solution is quickly cooled to room temperature to obtain the original solution of blue light nanosheets.
[0017] Furthermore, step S4 specifically includes:
[0018] Alkaline earth metal halide salts, oleic acid and octadecene are mixed and stirred at a certain temperature T5 for a certain time to obtain a clear solution C. Then, a certain amount of solution C and a certain amount of sulfonic acid ligand are added to the original solution of blue light nanosheets and stirred at a certain temperature T6 for a certain time to obtain a blue light nanosheet solution with high fluorescence quantum yield.
[0019] Furthermore, step S5 specifically includes:
[0020] A pre-set amount of antisolvent was added to the solution prepared in S4 and centrifuged. The resulting precipitate was then added back to the solvent for further dispersion. This process was repeated multiple times to thoroughly remove reaction waste generated during the synthesis of the nanosheets, ultimately resulting in clean, high-fluorescence quantum-yield blue perovskite nanosheets.
[0021] Furthermore, in step S1,
[0022] Salt A is one or more of the following: cesium carbonate, cesium nitrate, cesium vanadate, cesium oxalate, cesium chromate, cesium permanganate, cesium dichromate, cesium borate, cesium silicate, cesium sulfite, cesium tungstate, cesium molybdate, cesium dihydrogen phosphate, cesium oleate, cesium propionate, cesium butyrate, cesium citrate, cesium sulfate, and cesium tartrate; the organic ligand is one or more of the following: octanoic acid, oleic acid, stearic acid, caprylic acid, and trioctylphosphine oxide; the non-coordinating solvent is octadecene. The temperature T1 is 90–150℃; the stirring time is 30–200 min; the stirring speed is 200–800 rpm. The concentration of precursor solution A is 0.0108–0.8235 g / mL.
[0023] Furthermore, in step S2,
[0024] Lead halide is one or both of lead bromide and lead chloride; the non-coordinating solvent is octadecene; the organic cationic ligand is one or more of oleic acid, stearic acid, oxalic acid, mercaptopropionic acid, dodecyl mercaptoacetic acid, undecenoic acid, octanoic acid, and trioctylphosphine oxide; the organic anionic ligand can be, but is not limited to, one or more of oleylamine, dodecylamine, hexadecylamine, trioctylamine, tributylamine, trioctylphosphine, and octylamine; the vacuum degree is 0.6–50 Pa, the temperature T2 is 60–130 °C; the volume ratio of organic anionic ligand to organic cationic ligand is 0.2–1.5:1, the volume ratio of organic anionic ligand to non-coordinating solvent is 0.23–1.8:1; the temperature T3 is 140–250 °C, the stirring time is 20–150 min, and the concentration of precursor solution B is 0.0032–0.9732 g / mL.
[0025] Furthermore, in step S3,
[0026] Temperature T4 is 130–220℃; stirring speed is 300–1200 rpm; peristaltic pump flow rate is 0.002–32 ml / h; reaction time is 20 min–48 h.
[0027] Furthermore, in step S4,
[0028] The alkaline earth metal halide is one or more of calcium chloride, magnesium chloride, strontium chloride, barium chloride, calcium bromide, magnesium bromide, strontium bromide, and barium bromide; the temperature T5 is 60–150℃; the stirring time at temperature T5 is 30–300 min; the sulfonic acid ligand is sodium benzenesulfonate, p-toluenesulfonic acid, 2-naphthalenesulfonic acid, 3-amino-4-methylbenzenesulfonic acid, aminomethanesulfonic acid, 2-amino-3,5-dimethylbenzenesulfonic acid, aminomethanesulfonic acid, 4-dodecylbenzenesulfonic acid, or 2-sulfonicoterephthalic acid. One or more of the following: isophthalic acid-5-sulfonic acid, 1,3,5-benzenetrisulfonic acid, 4-chlorobenzenesulfonic acid, 2-carboxybenzenesulfonic acid, 3-carboxybenzenesulfonic acid, 4-aminobenzenesulfonic acid, 4-sulfonylbenzoic acid, and 1-naphthalenesulfonic acid; temperature T6 is room temperature to 180℃; stirring time at temperature T6 is 20 to 240 min; weight ratio of alkaline earth metal halide salt to sulfonic acid ligand is 0.25 to 2.3:1; weight ratio of alkaline earth metal halide salt to lead halide is 0.02 to 0.65:1.
[0029] Furthermore, in step S5,
[0030] The volume ratio of the antisolvent to the solvent is 0.2–2:1, and the volume ratio of the antisolvent to the blue nanosheet solution is 0.5–1.8:1; the antisolvent is ethyl acetate; the solvent is one of toluene, n-hexane, cyclohexane, benzene, or octane; the centrifugation speed is 800 rpm–10000 rpm; and the centrifugation time is 3 min–30 min.
[0031] Compared with the prior art, this patent application has the following advantages:
[0032] 1. Enhanced structural stability: The structure of nanosheets is relatively more stable. Traditional perovskite quantum dots, due to their high surface energy and small size, are prone to aggregation and Ostwald ripening, resulting in poor stability. The larger planar structure of perovskite nanosheets, however, reduces the impact of these instabilities to some extent. For example, during long-term use, perovskite nanosheets can better maintain their optical properties and structural integrity.
[0033] 2. Enhanced Resistance to External Interference: Perovskite nanosheets exhibit better stability against external factors such as light, heat, and air. In contrast, traditional monodisperse perovskite quantum dots are susceptible to photodegradation under light exposure, easily oxidized in air, and are more sensitive to heat, potentially experiencing performance degradation or even structural damage at higher temperatures. Due to their relatively stable structure and surface properties, perovskite nanosheets possess stronger resistance to these external interference factors. For example, in applications in outdoor or complex environments, perovskite nanosheets offer significant advantages.
[0034] 3. Modifiable Surface Properties: The surface of perovskite nanosheets is more easily chemically modified. By introducing different ligands or functional groups, their surface properties can be altered, thereby modulating their interaction with the surrounding environment and their optical properties. This surface modifiability provides more possibilities for further optimizing the performance of perovskite nanosheets and expanding their application range. For example, surface modification can improve their dispersibility in specific solvents or matrices and enhance their compatibility with other materials.
[0035] 4. Precise control over size and thickness: By changing the synthesis conditions, the size and thickness of perovskite nanosheets can be controlled relatively precisely, thereby achieving fine adjustment of their optical properties. For example, perovskite nanosheets with specific emission wavelengths can be synthesized according to different application requirements, satisfying the precise control of different colors of light, which is of great value in fields such as multicolor displays and optical communications. In contrast, the precision and range of size control of traditional monodisperse perovskite quantum dots may be relatively limited. Attached Figure Description
[0036] Figure 1 Mg:CsPbBr is used in the preparation method of ultra-large blue perovskite nanosheets with high fluorescence quantum yield according to the present invention. 3-x Cl x Fluorescence quantum yield of ultra-large blue light nanosheets;
[0037] Figure 2 Mg:CsPbBr is used in the preparation method of ultra-large blue perovskite nanosheets with high fluorescence quantum yield according to the present invention. 3-x Cl x Transmission electron microscopy morphology of ultra-large blue light nanosheets;
[0038] Figure 3 Mg:CsPbBr is used in the preparation method of ultra-large blue perovskite nanosheets with high fluorescence quantum yield according to the present invention. 3-x Cl x Magnified transmission electron microscope image of the ultra-large blue light nanosheets;
[0039] Figure 4 Mg:CsPbBr is used in the preparation method of ultra-large blue perovskite nanosheets with high fluorescence quantum yield according to the present invention. 3-x Cl x Fluorescence image of ultra-large blue light nanosheets;
[0040] Figure 5 Mg:CsPbBr is used in the preparation method of ultra-large blue perovskite nanosheets with high fluorescence quantum yield according to the present invention. 3-x Cl x Absorption diagram of ultra-large blue light nanosheets. Detailed Implementation
[0041] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0042] Example 1
[0043] A method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield includes the following steps:
[0044] S1: Preparation of precursor solution A
[0045] 0.45 g cesium carbonate, 1.5 mL oleic acid, 0.7 mL octanoic acid and 10 mL octadecene were thoroughly mixed, heated to 130 °C and stirred for 90 min at a stirring speed of 500 rpm to obtain a clear and transparent cesium precursor solution with a concentration of 0.0368 g / mL.
[0046] S2: Preparation of precursor solution B
[0047] 0.105 g lead chloride, 0.032 g lead bromide and 10 mL octadecene were mixed, vacuumed to 20 Pa, and heated to 120 °C. Then 1.5 mL oleic acid, 1.5 mL oleylamine and 2 mL trioctylphosphine were added to the solution. The temperature was then raised to 170 °C and stirred at this temperature for 30 min to obtain a clear and transparent lead halide precursor solution with a concentration of 0.0091 g / mL.
[0048] S3: The original solution for synthesizing nanosheets
[0049] Precursor solution B was heated to 170℃ and stirred at 300 rpm. Then, precursor solution A was injected into precursor solution B at a rate of 2.4 mL / h using a peristaltic pump. The reaction was carried out for 20 min, and then the solution was quickly cooled to room temperature to obtain the original solution of blue nanosheets.
[0050] S4: Passivation of nanosheet surface defects
[0051] 0.1 g magnesium chloride, 2 mL oleic acid, and 10 mL octadecene were mixed and stirred at 140 °C for 30 min to obtain a clear solution C. Then, 2 mL of solution C and 0.15 g of 2-carboxybenzenesulfonic acid were added to blue light nanosheets, and the mixture was stirred at 140 °C for 120 min to obtain blue light Mg:CsPbBr with high fluorescence quantum yield. 3-x Cl x Nanosheet solution;
[0052] S5: Purified Nanosheets
[0053] Take 5 mL of the solution prepared by L4, add 10 mL of ethyl acetate, and centrifuge at 5000 rpm for 5 min. Then, add the obtained precipitate to n-hexane for further dispersion; add ethyl acetate to the solution again, centrifuge, and then add the obtained precipitate to n-hexane for further dispersion. Finally, clean blue Mg:CsPbBr was successfully obtained. 3-x Cl x Nanosheets.
[0054] First, the fluorescence quantum yield of the nanosheets was characterized. It was found that the initial fluorescence quantum yield of the synthesized blue nanosheets was 67.1%. After modification with magnesium chloride and 2-carboxybenzenesulfonic acid, the fluorescence quantum yield increased to 93.6%. Figure 1 (This will then be achieved through analysis of CsPbBr) 1-x Cl x TEM characterization of the blue nanosheets revealed that they were square with side lengths of 200–500 nm. Figure 2 3). Fluorescence spectroscopy characterization revealed that Mg:CsPbBr 3-x Cl x The fluorescence peak of the nanosheet is at 456 nm, and the full width at half maximum (FWHM) is 35 nm. Figure 4 This demonstrates Mg:CsPbBr 3-x Cl x Nanosheets can serve as excellent materials for blue light illumination or displays, with absorption peaks at 410 nm and 425 nm. Figure 5 ).
[0055] Example 2
[0056] A method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield includes the following steps:
[0057] S1: Preparation of precursor solution A
[0058] 0.25 g cesium carbonate, 0.15 g cesium nitrate, 1.5 mL oleic acid, 0.9 mL octanoic acid and 10 mL octadecene were thoroughly mixed, heated to 140 °C, and stirred for 120 min at a stirring speed of 500 rpm to obtain a clear and transparent cesium precursor solution with a concentration of 0.0322 g / mL.
[0059] S2: Preparation of precursor solution B
[0060] 0.138 g of lead bromide was mixed with 10 mL of octadecene, the vacuum was drawn to 20 Pa, the temperature was raised to 120 °C, and then 1.5 mL of oleic acid and 1.5 mL of oleylamine were added to the solution. The temperature was then raised to 170 °C and stirred at this temperature for 30 min to obtain a clear and transparent lead halide precursor solution with a concentration of 0.0106 g / mL.
[0061] S3: The original solution for synthesizing nanosheets
[0062] Precursor solution B was heated to 130℃ and stirred at 500 rpm. Then, precursor solution A was injected into precursor solution B at a rate of 1.8 mL / h using a peristaltic pump. The reaction was carried out for 40 min, and then the solution was quickly cooled to room temperature to obtain the original solution of CsPbBr3 perovskite nanosheets.
[0063] S4: Passivation of nanosheet surface defects
[0064] 0.1 g calcium chloride, 2 mL oleic acid and 10 mL octadecene were mixed and reacted at 140 °C for 30 min to obtain a clear solution C. Then, 2 mL of solution C and 0.3 g of 2-carboxybenzenesulfonic acid were added to the original solution of perovskite nanosheets and stirred at 140 °C for 120 min to obtain a blue Ca:CsPbBr3 nanosheet solution with high fluorescence quantum yield.
[0065] S5: Purified Nanosheets
[0066] Take 5 mL of the solution prepared by S4, add 10 mL of ethyl acetate to it, and centrifuge at 5000 rpm for 5 min. Then, add the obtained precipitate to n-hexane for further dispersion, add ethyl acetate to the solution again, centrifuge, and then add the obtained precipitate to n-hexane for further dispersion. Finally, clean blue Ca:CsPbBr3 nanosheets were successfully obtained.
[0067] Example 3
[0068] A method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield includes the following steps:
[0069] S1: Preparation of precursor solution A
[0070] 0.35 g cesium nitrate, 1.5 mL oleic acid, 0.5 mL octanoic acid and 10 mL octadecene were thoroughly mixed, heated to 150 °C and stirred for 150 min at a stirring speed of 500 rpm to obtain a clear and transparent cesium precursor solution with a concentration of 0.0291 g / mL.
[0071] S2: Preparation of precursor solution B
[0072] 0.1408 g of lead chloride was mixed with 10 mL of octadecene, the vacuum was drawn to 20 Pa, the temperature was raised to 120 °C, and then 1 mL of oleic acid, 0.8 mL of oleylamine and 2.4 mL of trioctylphosphine were added to the solution. The temperature was then raised to 180 °C and stirred at this temperature for 60 min to obtain a clear and transparent lead chloride precursor solution with a concentration of 0.0099 g / mL.
[0073] S3: The original solution for synthesizing nanosheets
[0074] Precursor solution B was heated to 200℃ and stirred at 800 rpm. Then, precursor solution A was injected into precursor solution B at a rate of 3.6 mL / h using a peristaltic pump. The reaction was carried out for 60 min, and then the solution was quickly cooled to room temperature to obtain the original solution of CsPbCl3 perovskite nanosheets.
[0075] S4: Passivation of nanosheet surface defects
[0076] 0.1 g of strontium chloride, 3 mL of oleic acid and 8 mL of octadecene were mixed and reacted at 120 °C for 30 min to obtain a clear solution C. Then, 2 mL of solution C and 0.2 g of 4-aminobenzenesulfonic acid were added to the original solution of perovskite nanosheets and stirred at 120 °C for 240 min to obtain a blue Sr:CsPbCl3 nanosheet solution with high fluorescence quantum yield.
[0077] S5: Purified Nanosheets
[0078] Take 2.4 mL of the solution prepared by S4, add 5 mL of ethyl acetate to it, and centrifuge at 6000 rpm for 5 min. Then, add the obtained precipitate to n-hexane for further dispersion, add ethyl acetate to the solution again, centrifuge, and then add the obtained precipitate to n-hexane for further dispersion. Finally, clean blue Sr:CsPbCl3 nanosheets were successfully obtained.
Claims
1. A method for preparing ultra-large blue perovskite nanosheets with high fluorescence quantum yield, characterized in that, Includes the following steps: S1: Preparation of precursor solution A 0.45 g cesium carbonate, 1.5 mL oleic acid, 0.7 mL octanoic acid and 10 mL octadecene were thoroughly mixed, heated to 130 °C and stirred for 90 min at a stirring speed of 500 rpm to obtain a clear and transparent cesium precursor solution with a concentration of 0.0368 g / mL. S2: Preparation of precursor solution B 0.105 g lead chloride, 0.032 g lead bromide and 10 mL octadecene were mixed, vacuumed to 20 Pa, and heated to 120 °C. Then 1.5 mL oleic acid, 1.5 mL oleylamine and 2 mL trioctylphosphine were added to the solution. The temperature was then raised to 170 °C and stirred at this temperature for 30 min to obtain a clear and transparent lead halide precursor solution with a concentration of 0.0091 g / mL. S3: The original solution for synthesizing nanosheets Precursor solution B was heated to 170℃ and stirred at 300 rpm. Then, precursor solution A was injected into precursor solution B at a rate of 2.4 mL / h using a peristaltic pump. The reaction was allowed to proceed for 20 min. The solution was then rapidly cooled to room temperature to obtain the original solution of blue nanosheets. S4: Passivation of nanosheet surface defects 0.1 g magnesium chloride, 2 mL oleic acid and 10 mL octadecene were mixed and stirred at 140 °C for 30 min to obtain a clear solution C. Then, 2 mL of solution C and 0.15 g of 2-carboxybenzenesulfonic acid were added to the original solution of blue light nanosheets and stirred at 140 °C for 120 min to obtain a blue light Mg:CsPbBr3-xClx nanosheet solution with high fluorescence quantum yield. S5: Purified Nanosheets Take 5 mL of the solution prepared by LS4, add 10 mL of ethyl acetate to it, and centrifuge at 5000 rpm for 5 min. Then, add the obtained precipitate to n-hexane for further dispersion. Add ethyl acetate to the solution again, centrifuge, and then add the obtained precipitate to n-hexane for further dispersion to obtain clean blue Mg:CsPbBr3-xClx nanosheets.
Citation Information
Patent Citations
High-performance blue-light perovskite nanosheet and preparation method thereof
CN118599532A