Thermoplastic elastomer composite material, electronic cigarette component and method for preparing electronic cigarette component

By using retractable electronic cigarette components made of thermoplastic elastomer composite materials, the existing problems of fixed lengths of electronic cigarettes and unenvironmental materials are solved, and an efficient solution for easy storage and environmental protection is achieved.

CN119463521APending Publication Date: 2025-02-18DONGGUAN ZHENGXI PRECISION MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411616343.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-13
Publication Date
2025-02-18

AI Technical Summary

Technical Problem

The existing electronic cigarette poles and cigarette holders are made of conventional plastic, which makes it difficult to store in a fixed length and is not conducive to recycling.

Method used

Electronic cigarette components made of thermoplastic elastomer composite materials, including the suction nozzle and shell part, improve the elasticity and scalability of the material through specific raw material composition and preparation methods.

Benefits of technology

It realizes the retractable structure of electronic cigarette components, which is easy to store, while improving the environmental protection and recycling value of the materials, and enhancing the user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119463521A_ABST
    Figure CN119463521A_ABST
Patent Text Reader

Abstract

The invention discloses a component of an electronic cigarette. The component is made of a thermoplastic elastomer composite material. The components are a suction nozzle and an electronic cigarette shell part; the invention further discloses a thermoplastic elastomer composite material of an electronic cigarette component. The thermoplastic elastomer composite material comprises plant composite powder, the plant composite powder is a mixture of bamboo powder, hemp tree powder, paper mulberry powder, corn flour, lignin, cellulose, terpenoids, tannin, a starch extract and a castor oil extract; the invention further discloses a preparation method of the electronic cigarette component. According to the electronic cigarette shell part, at least three shells are connected in a sleeved mode and can stretch out and draw back, and a telescopic structure is formed; the cigarette rod and the cigarette holder are made of the environment-friendly thermoplastic elastomer composite material, so that the experience feeling of the cigarette holder and the mouth can be improved, and the cigarette holder and the mouth can be conveniently recycled in the future; the cigarette rod and the cigarette holder are of the telescopic structure in mutual sliding and sleeving connection, and storage of the electronic cigarette when the electronic cigarette is not used is better utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic cigarettes, and in particular to a thermoplastic elastomer composite material, an electronic cigarette component and a method for preparing the electronic cigarette component. Background Art

[0002] Due to the strengthening of the national anti-smoking propaganda and the improvement of people's health awareness, electronic cigarettes are being used more and more widely as a substitute for traditional tobacco. Electronic cigarettes generally include a cigarette rod and a mouthpiece. A battery is set in the cigarette rod, and an atomizer is installed in the mouthpiece. The atomizer is electrically connected to the cigarette rod. An oil cup is provided in the mouthpiece for holding the smoke liquid. When a person starts to smoke from the mouthpiece, the smoke liquid slowly flows into the atomizer, and the atomizer wire in the atomizer absorbs the smoke liquid. The control circuit board in the cigarette rod senses the current and controls the heating device at the atomizer wire to atomize the smoke liquid to form smoke, which is inhaled through the mouthpiece cover. This is the principle of electronic cigarettes. In the prior art, electronic cigarettes are composed of a cigarette rod and a mouthpiece fixedly connected, thereby forming a fixed length, which is not convenient for further storage. At the same time, the materials of the cigarette rod and the mouthpiece are made of conventional plastics, and the experience of the mouthpiece part and the mouth part contacting are intertwined, which is not conducive to future recycling and reuse. Summary of the invention

[0003] The present invention aims at the above problems and proposes a thermoplastic elastomer composite material, an electronic cigarette component and a method for preparing the electronic cigarette component to solve the above problems.

[0004] In order to achieve the above technical purpose, the present invention adopts a component of an electronic cigarette, which is made of a thermoplastic elastomer composite material; the component is a mouthpiece and an electronic cigarette shell;

[0005] The thermoplastic elastomer composite material is composed of the following raw materials by weight:

[0006] 20-40 parts of main material;

[0007] 15-25 parts of foaming agent;

[0008] 2-4 parts of additives;

[0009] The auxiliary agent includes a plasticizer, a heat stabilizer, an antioxidant, a flame retardant, a foaming agent, an antistatic agent, a mildew preventer, and a colorant. The components in the auxiliary agent are specifically as follows by weight:

[0010] 1-3 parts of plasticizer;

[0011] Heat stabilizer 0.8-1 part;

[0012] Antioxidant 0.4-0.6 parts;

[0013] Flame retardant 0.4-0.8 parts;

[0014] 1-2 parts of foaming agent;

[0015] Antistatic agent 0.2-0.6 parts;

[0016] 0.6-0.9 parts of mildew inhibitor;

[0017] 1-3 parts of colorant;

[0018] The main material is thermoplastic elastomer TPE and plant composite powder.

[0019] The present invention then discloses a thermoplastic elastomer composite material for electronic cigarette components, wherein the plant composite powder is a mixture of bamboo powder, hemp tree powder, paper mulberry powder, corn powder, lignin, cellulose, terpenoids, tannin, starch extract and castor oil extract.

[0020] As a preferred embodiment of the present invention, the mesh size of the plant composite powder is 300-400 meshes.

[0021] As a further preferred embodiment of the present invention, the molecular weight of the thermoplastic elastomer composite material is 120-170 kDa, the tensile strength can reach 25-35 MPa, the elongation at break is about 1500%, and the thermal decomposition temperature is greater than or equal to 400°C.

[0022] The present invention then discloses a method for preparing the electronic cigarette component, which specifically comprises the following steps:

[0023] Mixing: weigh 20-40 parts of the main material, 15-20 parts of the foaming agent and 2-4 parts of the auxiliary agent, and mix them thoroughly;

[0024] Preparation: Install the mold on the injection molding machine and adjust the mold temperature; the mold temperature is 50℃-70℃;

[0025] Mold closing: closing the mold;

[0026] Injection: Inject the uniformly mixed main material, foaming agent and auxiliary agent into the above mold at the set injection pressure and injection temperature; the set injection pressure is 50MPa-70Mpa, and the injection temperature is 170-220℃;

[0027] Pressure holding and cooling: The melted material is solidified under the set pressure holding. After the pressure holding is completed, it is gradually cooled in the mold.

[0028] The cooling time in the mold is 15 seconds to 20 seconds;

[0029] Mold opening: the mold is opened and the electronic cigarette parts are taken out;

[0030] As a further preferred embodiment of the present invention, at least three shells of the electronic cigarette shell part are sleeved and retractable, forming a retractable structure;

[0031] The telescopic structure specifically includes: a first shell, a second shell and a third shell, the inner wall of the first shell is provided with a first slideway; the outer wall of the second shell is provided with a first slider that can slide left and right on the first slideway, and the inner wall of the second shell is provided with a second slideway; the outer wall of the third shell is provided with a second slider that can slide left and right on the second slideway; thus, a telescopic shell structure composed of the first shell, the second shell and the third shell is formed.

[0032] After adopting the above materials, structures and preparation methods, the present invention has the following advantages:

[0033] The cigarette rod and the cigarette holder of the present invention are made of an environmentally friendly thermoplastic elastomer composite material, which can not only improve the experience of the cigarette holder and the mouth, but also facilitate future recycling;

[0034] The cigarette rod and the cigarette holder of the present invention are in a telescopic structure that are slidably sleeved with each other, so that the electronic cigarette can be stored more conveniently when not in use. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Shown is a schematic diagram of the overall structure of the present invention;

[0036] Among them, 1. first outer shell; second outer shell; third outer shell; 4. first slideway; 5. first slider; 6. second slideway; 7. second slider. DETAILED DESCRIPTION

[0037] In order to make the purpose and technical solution of the present invention clearer, the present invention is further described below in conjunction with the accompanying drawings and by selecting some data as examples. It should be understood that the selected data here are only used to assist in explaining the present invention and are not used to limit the present invention.

[0038] Combination Figure 1 It can be seen that a component of an electronic cigarette is made of a thermoplastic elastomer composite material; the component is a mouthpiece and an electronic cigarette shell part; that is, a cigarette rod and a cigarette mouthpiece part.

[0039] In the present invention, the thermoplastic elastomer composite material is composed of the following raw materials by weight:

[0040] 20-40 parts of main material;

[0041] 15-25 parts of foaming agent;

[0042] 2-4 parts of additives;

[0043] In the present invention, the auxiliary agent includes a plasticizer, a heat stabilizer, an antioxidant, a flame retardant, a foaming agent, an antistatic agent, a mildew preventer, and a colorant. The components in the auxiliary agent are specifically as follows by weight:

[0044] 1-3 parts of plasticizer;

[0045] Heat stabilizer 0.8-1 part;

[0046] Antioxidant 0.4-0.6 parts;

[0047] Flame retardant 0.4-0.8 parts;

[0048] 1-2 parts of foaming agent;

[0049] Antistatic agent 0.2-0.6 parts;

[0050] 0.6-0.9 parts of mildew inhibitor;

[0051] 1-3 parts of colorant;

[0052] The main materials of the invention are thermoplastic elastomer TPE and plant composite powder.

[0053] The present invention then discloses a thermoplastic elastomer composite material for electronic cigarette components, wherein the plant composite powder is a mixture of bamboo powder, hemp powder, paper mulberry powder, corn powder, lignin, cellulose, terpenoids, tannin, starch extract and castor oil extract.

[0054] In the present invention, the preferred mesh size of the plant composite powder is 300-400 meshes.

[0055] In the present invention, the molecular weight of the preferred thermoplastic elastomer composite material is 120-170 kDa, the tensile strength can reach 25-35 MPa, the elongation at break is about 1500%, and the thermal decomposition temperature is greater than or equal to 400°C.

[0056] The present invention then discloses a method for preparing the electronic cigarette component, which specifically comprises the following steps:

[0057] Mixing: weigh 20-40 parts of the main material, 15-20 parts of the foaming agent and 2-4 parts of the auxiliary agent, and mix them thoroughly;

[0058] Preparation: Install the mold on the injection molding machine and adjust the mold temperature; the mold temperature is 50℃-70℃; Mold closing: close the mold;

[0059] Injection: Inject the uniformly mixed main material, foaming agent and auxiliary agent into the above mold at the set injection pressure and injection temperature; the set injection pressure is 50MPa-70Mpa, and the injection temperature is 170-220℃;

[0060] Pressure holding and cooling: The melted material is solidified under the set pressure holding. After the pressure holding is completed, it is gradually cooled in the mold.

[0061] The cooling time in the mold is 15 seconds to 20 seconds;

[0062] Mold opening: the mold is opened and the electronic cigarette parts are taken out;

[0063] Depend on Figure 1 It can be seen that at least three shells of the electronic cigarette shell part of the present invention are sleeved and retractable, forming a retractable structure;

[0064] The telescopic structure specifically comprises: a first shell 1, a second shell 2 and a third shell 3, wherein the first shell 1 is usually used as the mouthpiece part of the electronic cigarette.

[0065] A first slideway 4 is provided on the inner wall of the first shell 1; a first slider 5 capable of sliding left and right on the first slideway 4 is provided on the outer wall of the second shell 2, and a second slideway 6 is provided on the inner wall of the second shell 2; a second slider 7 capable of sliding left and right on the second slideway 6 is provided on the outer wall of the third shell 3; thus, the first slideway 4 and the first slider 5 are slidably connected, and the second slideway 6 and the second slider 7 are slidably connected, so as to form a telescopic shell structure composed of the first shell 1, the second shell 2 and the third shell 3.

[0066] The present invention is further described below with reference to several preferred embodiments.

[0067] Example 1

[0068] A component of an electronic cigarette, which is made of a thermoplastic elastomer composite material; the component is a mouthpiece and an electronic cigarette shell part, namely a cigarette rod and a cigarette mouthpiece part.

[0069] In the present invention, the thermoplastic elastomer composite material is composed of the following raw materials by weight:

[0070] 20 copies of main materials;

[0071] 15 parts of foaming agent;

[0072] 2 parts of auxiliary agent;

[0073] The auxiliary agent of the present invention includes a plasticizer, a heat stabilizer, an antioxidant, a flame retardant, a foaming agent, an antistatic agent, a mildewproof agent, and a colorant. The components in the auxiliary agent are specifically as follows by weight:

[0074] 1 part of plasticizer;

[0075] 0.8 parts of heat stabilizer;

[0076] 0.4 parts of antioxidant;

[0077] Flame retardant 0.4 parts;

[0078] 1 part of foaming agent;

[0079] 0.2 parts of antistatic agent;

[0080] 0.6 parts of mildew inhibitor;

[0081] 1 part of colorant;

[0082] The main materials of the invention are thermoplastic elastomer TPE and plant composite powder.

[0083] The present invention then discloses a thermoplastic elastomer composite material for electronic cigarette components, wherein the plant composite powder is a mixture of bamboo powder, hemp powder, paper mulberry powder, corn powder, lignin, cellulose, terpenoids, tannin, starch extract and castor oil extract.

[0084] In the present invention, the preferred mesh size of the plant composite powder is 300 meshes.

[0085] In the present invention, the molecular weight of the preferred thermoplastic elastomer composite material is 120 kDa, the tensile strength can reach 25 MPa, the elongation at break is about 1500%, and the thermal decomposition temperature is greater than or equal to 400°C.

[0086] The present invention then discloses a method for preparing the electronic cigarette component, which specifically comprises the following steps:

[0087] Mixing: weigh 20 parts of the main material, 15 parts of the foaming agent and 2 auxiliary agents, and mix them thoroughly;

[0088] Preparation: Install the mold on the injection molding machine and adjust the mold temperature; the mold temperature is 50℃; Mold closing: close the mold;

[0089] Injection: Inject the uniformly mixed main material, foaming agent and auxiliary agent into the above mold at a set injection pressure and injection temperature; the set injection pressure is 50MPa, and the injection temperature is 170°C;

[0090] Pressure holding and cooling: The melted material is solidified under the set pressure holding. After the pressure holding is completed, it is gradually cooled in the mold.

[0091] The cooling time in the mold is 15 seconds;

[0092] Mold opening: The mold is opened and the electronic cigarette parts are taken out.

[0093] Example 2

[0094] A component of an electronic cigarette, which is made of a thermoplastic elastomer composite material; the component is a mouthpiece and an electronic cigarette shell part, namely a cigarette rod and a cigarette mouthpiece part.

[0095] In the present invention, the thermoplastic elastomer composite material is composed of the following raw materials by weight:

[0096] 40 copies of main materials;

[0097] 25 parts of foaming agent;

[0098] 4 parts of additives;

[0099] In the present invention, the auxiliary agent includes a plasticizer, a heat stabilizer, an antioxidant, a flame retardant, a foaming agent, an antistatic agent, a mildew preventer, and a colorant. The components in the auxiliary agent are specifically as follows by weight:

[0100] 3 parts of plasticizer;

[0101] 1 part of heat stabilizer;

[0102] 0.6 parts of antioxidant;

[0103] Flame retardant 0.8 parts;

[0104] 2 parts of foaming agent;

[0105] 0.6 parts of antistatic agent;

[0106] 0.9 parts of mildew inhibitor;

[0107] 3 parts of colorant;

[0108] The main materials of the invention are thermoplastic elastomer TPE and plant composite powder.

[0109] The present invention then discloses a thermoplastic elastomer composite material for electronic cigarette components, wherein the plant composite powder is a mixture of bamboo powder, hemp powder, paper mulberry powder, corn powder, lignin, cellulose, terpenoids, tannin, starch extract and castor oil extract.

[0110] In the present invention, the preferred mesh size of the plant composite powder is 400 meshes.

[0111] In the present invention, the molecular weight of the preferred thermoplastic elastomer composite material is 170 kDa, the tensile strength can reach 35 MPa, the elongation at break is about 1500%, and the thermal decomposition temperature is greater than or equal to 400°C.

[0112] The present invention then discloses a method for preparing the electronic cigarette component, which specifically comprises the following steps:

[0113] Mixing: weigh 40 parts of the main material, 20 parts of the foaming agent and 4 auxiliary agents, and mix them thoroughly;

[0114] Preparation: Install the mold on the injection molding machine and adjust the mold temperature; the mold temperature is 70°C; Mold closing: close the mold;

[0115] Injection: Inject the uniformly mixed main material, foaming agent and auxiliary agent into the above mold at the set injection pressure and injection temperature; the set injection pressure is 70Mpa, and the injection temperature is 220℃;

[0116] Pressure holding and cooling: The melted material is solidified under the set pressure holding. After the pressure holding is completed, it is gradually cooled in the mold.

[0117] The cooling time in the mold is 20 seconds;

[0118] Mold opening: The mold is opened and the electronic cigarette parts are taken out.

[0119] Example 3

[0120] A component of an electronic cigarette, which is made of a thermoplastic elastomer composite material; the component is a mouthpiece and an electronic cigarette shell part, namely a cigarette rod and a cigarette mouthpiece part.

[0121] In the present invention, the thermoplastic elastomer composite material is composed of the following raw materials by weight:

[0122] 30 copies of main materials;

[0123] 20 parts of foaming agent;

[0124] 3 parts of additives;

[0125] In the present invention, the auxiliary agent includes a plasticizer, a heat stabilizer, an antioxidant, a flame retardant, a foaming agent, an antistatic agent, a mildew preventer, and a colorant. The components in the auxiliary agent are specifically as follows by weight:

[0126] 2 parts of plasticizer;

[0127] Heat stabilizer 0.9 parts;

[0128] 0.5 parts of antioxidant;

[0129] 0.6 parts of flame retardant;

[0130] 1.5 parts of foaming agent;

[0131] 0.4 parts of antistatic agent;

[0132] 0.7 parts of mildew inhibitor;

[0133] 1.5 parts of colorant;

[0134] The main materials of the invention are thermoplastic elastomer TPE and plant composite powder.

[0135] The present invention then discloses a thermoplastic elastomer composite material for electronic cigarette components, wherein the plant composite powder is a mixture of bamboo powder, hemp powder, paper mulberry powder, corn powder, lignin, cellulose, terpenoids, tannin, starch extract and castor oil extract.

[0136] In the present invention, the preferred mesh size of the plant composite powder is 350 meshes.

[0137] In the present invention, the molecular weight of the preferred thermoplastic elastomer composite material is 140 kDa, the tensile strength can reach 30 MPa, the elongation at break is about 1500%, and the thermal decomposition temperature is greater than or equal to 400°C.

[0138] The present invention then discloses a method for preparing the electronic cigarette component, which specifically comprises the following steps:

[0139] Mixing: weigh 30 parts of the main material, 17 parts of the foaming agent and 2-4 parts of the auxiliary agent, and mix them thoroughly;

[0140] Preparation: Install the mold on the injection molding machine and adjust the mold temperature; the mold temperature is 60°C; Mold closing: close the mold;

[0141] Injection: Inject the uniformly mixed main material, foaming agent and auxiliary agent into the above mold at the set injection pressure and injection temperature; the set injection pressure is 60MPa and the injection temperature is 190°C;

[0142] Pressure holding and cooling: The melted material is solidified under the set pressure holding. After the pressure holding is completed, it is gradually cooled in the mold.

[0143] The cooling time in the mold is 18 seconds;

[0144] Mold opening: The mold is opened and the electronic cigarette parts are taken out.

[0145] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A component of an electronic cigarette, characterized in that: The component is made of a thermoplastic elastomer composite material; the component is a mouthpiece and an electronic cigarette shell; The thermoplastic elastomer composite material is composed of the following raw materials by weight: 20-40 parts of main material; 15-25 parts of foaming agent; 2-4 parts of additives; The auxiliary agent includes a plasticizer, a heat stabilizer, an antioxidant, a flame retardant, a foaming agent, an antistatic agent, a mildew preventer, and a colorant. The components in the auxiliary agent are specifically as follows by weight: 1-3 parts of plasticizer; Heat stabilizer 0.8-1 part; Antioxidant 0.4-0.6 parts; Flame retardant 0.4-0.8 parts; 1-2 parts of foaming agent; Antistatic agent 0.2-0.6 parts; 0.6-0.9 parts of mildew inhibitor; 1-3 parts of colorant; The main material is thermoplastic elastomer TPE and plant composite powder.

2. A thermoplastic elastomer composite material for making the electronic cigarette component of claim 1, characterized in that: The plant composite powder is a mixture of bamboo powder, hemp powder, paper mulberry powder, corn powder, lignin, cellulose, terpenoids, tannin, starch extract and castor oil extract.

3. A thermoplastic elastomer composite material for making electronic cigarette components according to claim 2, characterized in that: The mesh size of the plant composite powder is 300-400 meshes.

4. A thermoplastic elastomer composite material for making electronic cigarette components according to claim 2, characterized in that: The molecular weight of the thermoplastic elastomer composite material is 120-170 kDa, the tensile strength can reach 25-35 MPa, the elongation at break is about 1500%, and the thermal decomposition temperature is greater than or equal to 400°C.

5. A method for preparing an electronic cigarette component according to claim 1, characterized in that: The following steps are involved: Mixing: weigh 20-40 parts of the main material, 15-20 parts of the foaming agent and 2-4 parts of the auxiliary agent, and mix them thoroughly; Preparation: Install the mold on the injection molding machine and adjust the mold temperature; the mold temperature is 50℃-70℃; Mold closing: closing the mold; Injection: The uniformly mixed main material, foaming agent and additives are injected into the Inject into the above mold; the set injection pressure is 50MPa-70Mpa, and the injection temperature is 170-220℃; Pressure holding and cooling: The melted material is solidified under the set pressure holding. After the pressure holding is completed, it is gradually cooled in the mold. The cooling time in the mold is 15 seconds to 20 seconds; Mold opening: The mold is opened and the electronic cigarette parts are taken out.

6. The component of an electronic cigarette according to claim 1, characterized in that: At least three shells of the electronic cigarette shell part are sleeved and retractable, forming a retractable structure; The telescopic structure specifically includes: a first shell, a second shell and a third shell, the inner wall of the first shell is provided with a first slideway; the outer wall of the second shell is provided with a first slider that can slide left and right on the first slideway, and the inner wall of the second shell is provided with a second slideway; the outer wall of the third shell is provided with a second slider that can slide left and right on the second slideway; thus, a telescopic shell structure composed of the first shell, the second shell and the third shell is formed.