A high ionic conductivity sulfide solid electrolyte, its preparation method, and its application

By adjusting the ratio of Li2S, GeS2, Sb2S3, Si, and LiI, Li(7-x)(GeSi)(1-x)/2SbxS5I sulfide solid electrolyte was prepared using ball milling and calcination. This solved the problem of low ionic conductivity in sulfide solid electrolytes of silver-germanium sulfide type, and realized a sulfide solid electrolyte with high ionic conductivity and excellent electrochemical performance, thus promoting its commercial application.

CN119495801BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311029610.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-15
Publication Date
2026-11-17
Estimated Expiration
2043-08-15

AI Technical Summary

Technical Problem

Existing sulfide solid electrolytes of silver-germanium sulfide type have low ionic conductivity, high preparation costs, and are difficult to industrialize. In addition, their rate capability and long-cycle performance are poor.

Method used

By adjusting the ratio of Li2S, GeS2, Sb2S3, Si, S, and LiI, a high-ionic-conductivity sulfide solid electrolyte was prepared using conventional ball milling and calcination methods. The electrolyte was designed with the general formula Li(7-x)(GeSi)(1-x)/2SbxS5I to increase the ionic radius, provide lithium-ion transport channels, and improve ionic conductivity.

Benefits of technology

A sulfide solid electrolyte with high ionic conductivity and excellent electrochemical performance was achieved, which improved the co-migration of lithium ions and the long cycle performance of the battery, and reduced the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119495801B_ABST
    Figure CN119495801B_ABST
Patent Text Reader

Abstract

This application discloses a high ionic conductivity sulfide solid electrolyte, its preparation method, and its application. The general formula of the high ionic conductivity sulfide solid electrolyte is Li. (7‑x) (GeSi) (1‑x) / 2Sb x S5I, where 1 / 3 ≤ x ≤ 1. This invention primarily improves the ionic conductivity and electrochemical performance of LPSI (lithium phosphosulfur iodide) sulfide solid electrolyte by adjusting the ratio of Li2S, GeS2, Sb2S3, Si, S, and LiI, thereby obtaining a sulfide solid electrolyte with high ionic conductivity and excellent electrochemical performance. This electrolyte, through the complete substitution of P by Ge, Si, and Sb, increases the ionic radius, providing a channel for lithium-ion transport and achieving synergistic lithium-ion migration and high ionic conductivity. The assembled all-solid-state battery exhibits extremely high capacity and excellent long-cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a high ionic conductivity sulfide solid electrolyte, its preparation method, and its application, belonging to the field of sulfide solid batteries. Background Technology

[0002] Currently, existing solid electrolytes are mainly classified into three types: oxide solid electrolytes, sulfide solid electrolytes, and polymer solid electrolytes. Sulfide solid electrolytes are considered to have the broadest industrialization prospects due to their high ionic conductivity and processing performance. The commercial application of sulfide solid electrolytes requires first meeting the prerequisite of high ionic conductivity. Currently reported LGPS and LSPSCl exhibit good ionic conductivity (~10 mS / cm). -1 However, its rate capability and long-cycle performance are poor. Its tetragonal structure has poor stability, requiring more pretreatment to achieve ideal electrochemical performance. In contrast, sulfide solid electrolytes of the silver-germanium sulfide type have a stable structure, good stability during battery cycling, and excellent rate capability, showing broad application prospects. However, the reported ionic conductivity of silver-germanium sulfide is currently low; therefore, silver-germanium sulfide solid electrolytes are still far from practical application.

[0003] In existing technologies, technicians have used methods such as high-energy ball milling and plasma to prepare corresponding solid electrolytes, but these methods are costly and difficult to industrialize. Therefore, there is an urgent need to find inexpensive, simple to prepare, and high-performance sulfide solid electrolytes with high ionic conductivity for application in lithium batteries. Summary of the Invention

[0004] To address the aforementioned problems with existing preparation techniques, the present invention aims to propose an effective method for producing high-ionic-conductivity sulfide solid electrolytes. This method involves the conventional ball milling and calcination of raw materials Li2S, P2S5, GeS2, Sb2S3, Si, S, and LiI to obtain high-ionic-conductivity sulfide solid electrolytes with excellent electrochemical performance, thereby promoting their commercialization.

[0005] According to one aspect of this application, a high ionic conductivity sulfide solid electrolyte is provided, characterized in that the general formula of the high ionic conductivity sulfide solid electrolyte is Li. (7-x) (GeSi) (1-x) / 2 Sb x S5I, where 1 / 3≤x≤1.

[0006] Optionally, the general formula of the high ionic conductivity sulfide solid electrolyte is Li (7-x) (GeSi) (1-x) / 2 Sb xS5I, where the value of x is selected from any value of 1 / 3, 1 / 2, 2 / 3, 1 or any value between any two of the above.

[0007] Optionally, the ionic conductivity of the high ionic conductivity sulfide solid electrolyte is 1×10⁻⁶. -3 ~2×10 - 2 S / cm.

[0008] Optionally, the ionic conductivity of the high ionic conductivity sulfide solid electrolyte is selected from 1×10⁻⁶. -3 S / cm, 2×10 -3 S / cm, 3×10 -3 S / cm, 2×10 -2 Any value in S / cm or the range between any two points mentioned above.

[0009] According to another aspect of this application, a method for preparing the high ionic conductivity sulfide solid electrolyte is provided, the method comprising:

[0010] A mixture containing Li2S, Sb2S3, S, and LiI is ball-milled and reacted to obtain the high ionic conductivity sulfide solid electrolyte.

[0011] Optionally, the mixture may also include GeS2 and Si.

[0012] Optionally, the molar ratio of Li2S, GeS2, Si, Sb2S3, S, and LiI is 2.5–3: 0–0.33: 0–0.33: 0.17–0.5: 1.05: 1.

[0013] Optionally, the ball mill rotates at a speed of 300 to 500 rpm and the milling time is 15 to 25 hours.

[0014] Optionally, the rotational speed of the ball mill is selected from any value among 300 rpm, 350 rpm, 400 rpm, 450 rpm, and 500 rpm, or a range between any two of the above points.

[0015] Optionally, the ball milling time is selected from any value among 15h, 17h, 20h, 22h, and 25h, or a range between any two of the above points.

[0016] Optionally, a pre-grinding process is performed before ball milling, wherein the pre-grinding speed is 100-300 rpm and the pre-grinding time is 1-2 hours.

[0017] Optionally, the pre-grinding speed is selected from any value among 100 rpm, 150 rpm, 200 rpm, 250 rpm, and 300 rpm, or a range between any two of the above points.

[0018] Optionally, the pre-grinding time is selected from any value among 1h, 1.2h, 1.5h, 2h, or a range between any two of the above points.

[0019] Optionally, the reaction temperature is 400–500°C, and the reaction time is 3–7 hours.

[0020] Optionally, the temperature of the reaction is selected from any value of 400℃, 420℃, 450℃, 480℃, 500℃ or a range between any two of the above points.

[0021] Optionally, the reaction time is selected from any value of 3h, 4h, 5h, 6h, 7h or a range between any two of the above points.

[0022] According to another aspect of this application, an application of the high ionic conductivity sulfide solid electrolyte described above in a sulfide solid battery is provided.

[0023] Optionally, the sulfide solid-state battery includes a positive electrode, a negative electrode, and a solid electrolyte;

[0024] The solid electrolyte is a sulfide solid electrolyte with high ionic conductivity.

[0025] The positive electrode is selected from LiNi. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 One of O2 and LiCoO2;

[0026] The negative electrode is selected from at least one of Li-In alloy, Li-Mg alloy, and Li-Sn alloy.

[0027] This application is achieved through the following technical solution:

[0028] A design scheme for a high ionic conductivity sulfide solid electrolyte includes the preparation of the high ionic conductivity sulfide solid electrolyte, the matching of positive and negative electrodes and their structural design.

[0029] The composite sulfide solid electrolyte is prepared by the following steps:

[0030] (1) Li2S, GeS2, Si, Sb2S3, S, and LiI in a molar ratio of 2.5-3:0-0.33:0-0.33:0.17-0.5:1.05:1 are placed in a ball mill jar and pre-milled at 100-300 rpm for 1-2 hours and ball-milled at 300-500 rpm for 15-25 hours to obtain an amorphous phase mixture of sulfide solid electrolyte. The mixture is then cold-pressed to obtain a blank, which is placed in a quartz tube and heated at room temperature to 400-500℃ for 3-7 hours. The temperature is then lowered to room temperature to obtain a ceramic phase high ionic conductivity sulfide solid electrolyte.

[0031] (2) Place 90-110 mg of solid electrolyte in a battery mold and press it under a pressure of 400-550 MPa for 1-3 minutes. The positive electrode is NCM811 (LiNi). 0.8 Co 0.1 Mn 0.1 O2), NCM622(LiNi) 0.6 Co 0.2 Mn 0.2 Press one of O2 or LCO (LiCoO2) under a pressure of 400-550 MPa for 1-3 minutes.

[0032] (3) Place one or more of the cut Li-In, Li-Mg or Li-Sn alloys as the negative electrode at the bottom of the battery mold, press it with a pressure of 20-50 MPa for 1-3 minutes, and finally test its electrochemical performance.

[0033] In step (2), the solid electrolyte is Li 20 / 3 (GeSi) 1 / 3 Sb 1 / 3 S5I, Li 19 / 3 (GeSi) 1 / 6 Sb 2 / 3 S5I, Li 13 / 2 (GeSi) 1 / 4 Sb 1 / 2 One of S5I and Li6(GeSi)0Sb1S5I.

[0034] This invention discloses a method for designing, preparing, and applying a high-ionic-conductivity sulfide solid-state electrolyte. This invention belongs to the field of sulfide solid-state batteries. The invention mainly improves the ionic conductivity and electrochemical performance of LPSI (lithium phosphosulfur iodide) with a sulfide-silver-germanium ore structure by adjusting the ratio of Li₂S, GeS₂, Sb₂S₃, Si, S, and LiI, thereby obtaining a high-ionic-conductivity sulfide solid-state electrolyte with excellent electrochemical performance. This electrolyte, through the complete substitution of P elements by Ge, Si, and Sb, increases the ionic radius, providing a channel for lithium-ion transport, resulting in the cooperative migration of lithium ions and high ionic conductivity. The assembled all-solid-state battery exhibits extremely high capacity and excellent long-cycle performance.

[0035] The beneficial effects that this application can produce include:

[0036] 1) The high ionic conductivity sulfide solid electrolyte provided in this application increases the ionic radius and improves the ionic conductivity of the sulfide solid electrolyte by completely replacing P with Ge, Si and Sb.

[0037] 2) The high ionic conductivity sulfide solid electrolyte provided in this application has the ability to improve the ionic conductivity of the sulfur-iodine solid electrolyte by adjusting the preparation conditions.

[0038] 3) The high ionic conductivity sulfide solid electrolyte provided in this application provides a channel for lithium-ion transport, resulting in the co-migration of lithium ions and high ionic conductivity, thereby improving electrochemical performance. Attached Figure Description

[0039] Figure 1 Li in Embodiment 1 of this application 20 / 3 (GeSi) 1 / 3 Sb 1 / 3 XRD pattern of S5I.

[0040] Figure 2 Li in Embodiment 1 of this application 20 / 3 (GeSi) 1 / 3 Sb 1 / 3 Enlarged XRD pattern of S5I.

[0041] Figure 3 This is an impedance curve of the high ionic conductivity sulfide solid electrolyte of Example 1 of this application.

[0042] Figure 4 This is a rate curve of the sulfide all-solid-state battery of Example 1 of this application.

[0043] Figure 5 This is a graph showing the long-cycle performance of the sulfide all-solid-state battery of Example 1 of this application. Detailed Implementation

[0044] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0045] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0046] This application uses a Zana electrochemical workstation for EIS impedance testing.

[0047] This application uses a blue electric tester to test the electrochemical performance of solid-state batteries.

[0048] Unless otherwise specified, all reagents or instruments used in this application are commercially available products.

[0049] In this application embodiment, room temperature refers to "25°C".

[0050] Example 1

[0051] A mixture of 0.651 g Li₂S, 0.2279 g GeS₂, 0.0468 g Si, 0.2831 g Sb₂S₃, 0.1683 g S, and 0.6692 g LiI (in a molar ratio of 2.83:0.33:0.33:0.17:1.05:1) was fed into a ball mill jar (ball-to-material ratio 20:1). The mixture was pre-milled at 100 rpm for 0.5 h and then ball-milled at 450 rpm for 20 h to obtain an amorphous mixture of sulfide solid electrolytes. This mixture was cold-pressed to obtain a green blank, which was then placed in a quartz tube and heated to 450 °C at room temperature for 5 h. After cooling to room temperature, a ceramic-phase high-ionic-conductivity sulfide solid electrolyte, Li₂S, was obtained. 20 / 3 (GeSi) 1 / 3 Sb 1 / 3 S5I. 100 mg of solid electrolyte was weighed and placed into a battery mold, pressed at 550 MPa for 1 min, with Li-In as the negative electrode and NCM811 as the positive electrode, and a long-cycle test was conducted at a current density of 0.1 C. The test showed that after 100 cycles, the battery capacity remained at 175 mAh g. -1 .like Figure 1 and Figure 2 The image shows Li 20 / 3 (GeSi) 1 / 3Sb 1 / 3 XRD pattern of S5I. From Figure 1 and Figure 2 As can be seen, the narrowest lattice spacing corresponds to the smallest unit cell and the highest lithium-ion concentration. From... Figure 3 The impedance curve shows a significant decrease in impedance and a significant increase in ionic conductivity. From... Figure 4 As can be seen from the rate performance diagram of the sulfide all-solid-state battery, it achieves good rate performance; from Figure 5As can be seen, the all-solid-state battery can operate stably for 300 cycles at a current of 0.5C at room temperature.

[0052] Example 2

[0053] A mixture of 0.632 g Li₂S, 0.171 g GeS₂, 0.0351 g Si, 0.4246 g Sb₂S₃, 0.1683 g S, and 0.6692 g LiI (in a molar ratio of 2.75:0.25:0.25:0.25:1.05:1) was fed into a ball mill jar (ball-to-material ratio 20:1). The mixture was pre-milled at 100 rpm for 0.5 h and then ball-milled at 450 rpm for 20 h to obtain an amorphous mixture of sulfide solid electrolytes. This mixture was cold-pressed to obtain a green blank, which was then placed in a quartz tube and heated to 450 °C at room temperature for 5 h. After cooling to room temperature, a ceramic-phase high-ionic-conductivity sulfide solid electrolyte, Li₂S, was obtained. 13 / 2 (GeSi) 1 / 4 Sb 1 / 2 S5I. 100 mg of solid electrolyte was weighed and placed into a battery mold, pressed at 550 MPa for 1 min, with Li-In as the negative electrode and NCM811 as the positive electrode, and a long-cycle test was conducted at a current density of 0.1 C. The test showed that after 100 cycles, the battery capacity remained at 168 mAh g. -1 .

[0054] Example 3

[0055] A mixture of 0.6127 g Li₂S, 0.114 g GeS₂, 0.0234 g Si, 0.5662 g Sb₂S₃, 0.1683 g S, and 0.6692 g LiI (in a molar ratio of 2.66:0.17:0.17:0.33:1.05:1) was fed into a ball mill jar (ball-to-material ratio 20:1). The mixture was pre-milled at 100 rpm for 0.5 h and then ball-milled at 450 rpm for 20 h to obtain an amorphous mixture of sulfide solid electrolytes. This mixture was cold-pressed to obtain a green blank, which was then placed in a quartz tube and heated to 450 °C at room temperature for 5 h. After cooling to room temperature, a ceramic-phase high-ionic-conductivity sulfide solid electrolyte, Li₂S, was obtained. 19 / 3 (GeSi) 1 / 6 Sb 2 / 3 S5I. 100 mg of solid electrolyte was weighed and placed into a battery mold, pressed at 550 MPa for 1 min, with Li-In as the negative electrode and NCM811 as the positive electrode, and a long-cycle test was conducted at a current density of 0.1 C. The test showed that the battery maintained a capacity of 163 mAh g after 100 cycles. -1 .

[0056] Example 4

[0057] A mixture of 0.574 g Li₂S, 0 g GeS₂, 0 g Si, 0.848 g Sb₂S₃, 0.1683 g S, and 0.6692 g LiI in a molar ratio of 2.5:0:0:0.5:1.05:1 was fed into a ball mill jar (ball-to-material ratio 20:1). The mixture was pre-milled at 100 rpm for 0.5 h and then ball-milled at 450 rpm for 20 h to obtain an amorphous mixture of sulfide solid electrolyte. This mixture was cold-pressed to obtain a preform, which was then placed in a quartz tube and heated to 450 °C at room temperature for 5 h. After cooling to room temperature, a ceramic-phase high-ionic-conductivity sulfide solid electrolyte, Li₆(GeSi)₀Sb₁S₅I, was obtained. 100 mg of the solid electrolyte was weighed and placed in a battery mold, pressed at 550 MPa for 1 min, and a long-cycle test was conducted using Li-In as the negative electrode, NCM811 as the positive electrode, and a current density of 0.1 C. The test showed that the battery maintained a capacity of 150mAh g after 100 cycles. -1 .

[0058] Comparative Example 1

[0059] A mixture of 0.670 g Li₂S, 0.285 g GeS₂, 0.058 g Si, 0.141 g Sb₂S₃, 0.1683 g S, and 0.6692 g LiI (in a molar ratio of 2.92:0.417:0.417:0.083:1.05:1) was fed into a ball mill jar (ball-to-material ratio 20:1). The mixture was pre-milled at 100 rpm for 0.5 h and then ball-milled at 450 rpm for 20 h to obtain an amorphous mixture of sulfide solid electrolytes. This mixture was cold-pressed to obtain a green blank, which was then placed in a quartz tube and heated to 450 °C at room temperature for 5 h. After cooling to room temperature, a ceramic-phase high-ionic-conductivity sulfide solid electrolyte, Li₂S₃, was obtained. 41 / 6 (GeSi) 5 / 12 Sb 1 / 6 S5I. 100 mg of solid electrolyte was weighed and placed into a battery mold, pressed at 550 MPa for 1 min, with Li-In as the negative electrode and NCM811 as the positive electrode, and a long-cycle test was conducted at a current density of 0.1 C. The test showed that the battery maintained a capacity of 80 mAh g after 100 cycles. -1 .

[0060] Comparative Example 2

[0061] A mixture of 0.551 g Li₂S, 0 g GeS₂, 0 g Si, 1.02 g Sb₂S₃, 0.202 g S, and 0.6692 g LiI (in a molar ratio of 2.4:0:0:0.6:1.26:1) was fed into a ball mill jar (ball-to-material ratio 20:1). The mixture was pre-milled at 100 rpm for 0.5 h and then ball-milled at 450 rpm for 20 h to obtain an amorphous mixture of sulfide solid electrolytes. This mixture was cold-pressed to obtain a green blank, which was then placed in a quartz tube and heated to 450 °C at room temperature for 5 h. After cooling to room temperature, a ceramic-phase high-ionic-conductivity sulfide solid electrolyte, Li, was obtained. 29 / 5 (GeSi)0Sb 6 / 5 S5I. 100 mg of solid electrolyte was weighed and placed into a battery mold, pressed at 550 MPa for 1 min, with Li-In as the negative electrode and NCM811 as the positive electrode, and a long-cycle test was conducted at a current density of 0.1 C. The test showed that the battery maintained a capacity of 20 mAh g after 100 cycles. -1 .

[0062] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A sulfide solid electrolyte with high ionic conductivity, characterized in that, The general formula of the high ionic conductivity sulfide solid electrolyte is Li (7-x) (GeSi) (1-x) / 2 Sb x S5I, where 1 / 3 ≤ x ≤ 2 / 3.

2. The high ionic conductivity sulfide solid electrolyte according to claim 1, characterized in that, The ionic conductivity of the high-ionic-conductivity sulfide solid electrolyte is 1×10⁻⁶. -3 ~2×10 -2 S / cm.

3. The method for preparing the high ionic conductivity sulfide solid electrolyte according to any one of claims 1 to 2, characterized in that, The preparation method includes: A mixture containing Li2S, Sb2S3, S, and LiI is ball-milled and reacted to obtain the high ionic conductivity sulfide solid electrolyte. The mixture also includes GeS2 and Si.

4. The preparation method according to claim 3, characterized in that, The molar ratio of Li2S, GeS2, Si, Sb2S3, S, and LiI is 2.5~3∶0~0.33∶0~0.33∶0.17~0.5∶1.05∶1.

5. The preparation method according to claim 3, characterized in that, The ball mill rotates at a speed of 300-500 rpm and the milling time is 15-25 hours.

6. The preparation method according to claim 3, characterized in that, Before ball milling, a pre-grinding process is performed. The pre-grinding speed is 100~300 rpm, and the pre-grinding time is 1~2 hours.

7. The preparation method according to claim 3, characterized in that, The reaction temperature is 400~500℃, and the reaction time is 3~7h.

8. The application of the high ionic conductivity sulfide solid electrolyte according to any one of claims 1 to 2 in sulfide solid batteries.

9. The application according to claim 8, characterized in that, The sulfide solid-state battery includes a positive electrode, a negative electrode, and a solid electrolyte; The solid electrolyte is a sulfide solid electrolyte with high ionic conductivity. The positive electrode is selected from LiNi. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 One of O2 and LiCoO2; The negative electrode is selected from at least one of Li-In alloy, Li-Mg alloy, and Li-Sn alloy.