A method for preparing a carbide-reinforced CoCrFeNi high-entropy alloy

By adding TiC to a CoCrFeNi high-entropy alloy and subjecting it to high-temperature melting, rolling, and annealing, a high-entropy alloy composed of an alloy matrix phase and multi-phase, multi-scale carbides was prepared, solving the problem of low strength and achieving excellent strength and toughness.

CN119710424BActive Publication Date: 2026-11-17WUHAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411914701.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-24
Publication Date
2026-11-17
Estimated Expiration
2044-12-24

AI Technical Summary

Technical Problem

CoCrFeNi high-entropy alloys have low strength, and existing methods offer limited improvement while reducing plasticity.

Method used

By adding hard TiC and employing high-temperature melting, rolling, and annealing, a high-entropy alloy composed of an alloy matrix phase and multi-phase, multi-scale carbides was prepared. The strength and toughness of the alloy were improved by using fine-grain strengthening and carbide second-phase strengthening.

Benefits of technology

It exhibits excellent room temperature strength and toughness, with a yield strength of 0.68–1.4 GPa, an ultimate tensile strength of 0.85–1.5 GPa, and an elongation of 1–22%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119710424B_ABST
    Figure CN119710424B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a carbide-reinforced CoCrFeNi high-entropy alloy, belonging to the field of metallic materials and processing technology. This invention involves adding hard TiC and preparing a high-entropy alloy composed of an alloy matrix phase and multi-phase, multi-scale carbides through high-temperature melting, rolling, and annealing. The rolling and annealing processes induce dynamic recrystallization of the matrix phase, precipitating fine and dispersed carbide particles. The combined strength and toughness of the alloy are improved through grain refinement and second-phase strengthening by the carbides, resulting in a high-entropy carbide-reinforced CoCrFeNi alloy with excellent strength and toughness, which is expected to be used in aerospace structural components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a high-entropy CoCrFeNi alloy reinforced with exhaust carbide, belonging to the field of metal materials and processing technology. Background Technology

[0002] Entropy alloys, composed of multiple principal elements, exhibit high mixing entropy and lattice distortion, displaying a series of excellent properties such as superior wear and corrosion resistance, high-temperature stability, and electrical and thermal conductivity. These superior properties make high-entropy alloys promising for broad industrial applications. CoCrFeNi high-entropy alloy is one of the earliest proposed and most studied alloys, possessing a face-centered cubic (FCC) single-phase structure. Its excellent room-temperature plasticity and slightly higher strength than traditional alloys have attracted great interest from researchers both domestically and internationally. However, with the deepening of research and the increasing demands of manufacturing for material properties, the low strength of CoCrFeNi high-entropy alloys has become increasingly prominent.

[0003] To strengthen CoCrFeNi high-entropy alloys, alloying, heat treatment, and mechanical hot deformation are commonly employed. Alloying forms solid solution elements or a second phase, thereby increasing the alloy's strength through solid solution strengthening or second-phase strengthening. He et al. prepared a CoCrFeNiNbx eutectic high-entropy alloy by adding Nb elements during smelting. This alloy exhibited a two-phase eutectic structure consisting of an FCC matrix and a lamellar Laves phase, demonstrating higher casting performance and strength compared to the CoCrFeNi alloy. However, due to the formation of the brittle Laves phase, the ductility of the eutectic alloy decreased by approximately 40% (He JY, Liu WH, Wang H., et al. Effects of Nb additions on the microstructure and mechanical property of CoCrFeNi high-entropy alloys. Intermetallics, 2015, 60: 1-8). High-hardness carbide phases are often introduced as second phases to improve the mechanical properties of high-entropy alloys. For example, Huang et al. added 10 vol.% TiC to CoCr3Fe5Ni alloy, and the yield strength of the alloy obtained by melting was increased by 30%, and the tensile strength was increased by 23%, to 401 MPa and 795 MPa, respectively, while the elongation was reduced to 17% (Huang S., Zhang J., Wu H., et al. Boosted mechanical properties of CoCr3Fe5Nihigh entropy alloy via in-situ TiC particles. Journal of Alloys and Compounds, 2023, 968:172051). The yield strength of the CoCrFeNiTiC alloy prepared by adding 5 vol% TiC to the CoCrFeNi alloy is increased to 550 MPa, while the elongation is reduced to 16% (Zhang J., Jia T., Qiu H., et al. Effect of cooling rate upon the microstructure and mechanical properties of in-situ TiC reinforced high entropy alloy CoCrFeNi. Journal of Materials Science & Technology, 2020, 42: 122-129).In summary, introducing a second phase through alloying or directly adding carbides can improve the strength of alloys, but the plasticity of the alloys is reduced and the strength improvement is limited. The yield strengths of TiC / CoCr3Fe5Ni and TiC / CoCrFeNi alloys are only about 400 MPa and 550 MPa, respectively.

[0004] Dual-phase high-entropy alloys are processed using rolling and annealing to improve their strength while maintaining good plasticity. For example, Hou et al. used rolling and annealing to process as-cast Al... 0.45 A CoCrFeNi dual-phase high-entropy alloy was cold-rolled 70% and annealed. After annealing, the matrix phase underwent dynamic recrystallization, and fine granular phases precipitated in the alloy. Under the effects of grain refinement strengthening and precipitation strengthening, the yield strength of the alloy increased from 209 MPa in the as-cast state to 727 MPa, and the elongation was 22% (Hou J., Wang Z., Shi X., et al. Strengthening of an Al 0.45 CoCrFeNi high-entropy alloy via in situfabricated duplex-structured composites. Journal of Materials Science, 2020, 55: 7894-7909. The rolling and annealing treatment of this dual-phase high-entropy alloy provides theoretical guidance for improving the strength of CoCrFeNi high-entropy alloys. Summary of the Invention

[0005] To address the low strength of CoCrFeNi high-entropy alloys, this invention proposes adding hard TiC and then processing it through high-temperature melting, rolling, and annealing to obtain a high-entropy alloy composed of an alloy matrix phase and multi-phase, multi-scale carbides. Rolling and annealing induce dynamic recrystallization of the matrix phase, precipitating fine, dispersed carbide particles. The combined strength and toughness of the alloy are improved through grain refinement and second-phase strengthening by the carbides, resulting in a carbide-reinforced CoCrFeNi high-entropy alloy with excellent strength and toughness.

[0006] To address the aforementioned technical problems, this invention provides a carbide-reinforced CoCrFeNi high-entropy alloy, wherein the alloy is composed of a face-centered cubic high-entropy alloy phase and a carbide phase; the high-entropy alloy phase is an FCC solid solution composed of Co, Cr, Fe, Ni, and Ti elements; and the carbide phase is (Cr, Co, Fe, Ni, Ti). 23 A mixture of C6 solid solution and (Ti,Cr,Co,Fe,Ni)C solid solution, (Cr,Co,Fe,Ni,Ti) 23The atomic ratio of Cr, Co, Fe, Ni, Ti, and C in C6 solid solution is (50-53): (9-10): (8-10): (5-8): (1-2): (21-23); the atomic ratio of Ti, Co, Fe, Ni, Cr, and C in (Ti,Cr,Co,Fe,Ni)C solid solution is (20-22): (8-10): (8-10): (7-9): (8-10): (43-45).

[0007] As an improvement to the above technical solution, the microstructure of the high-entropy alloy consists of a dendritic high-entropy alloy phase, interdendritic micron-sized carbide particles, and annealed micro-nano carbide particles, with good phase interface bonding.

[0008] A method for preparing a carbide-reinforced CoCrFeNi high-entropy alloy as described above comprises the following steps: weighing Co metal powder, Cr metal powder, Fe metal powder, Ni metal powder and TiC powder according to the atomic ratio of (0.95-1.05):(0.95-1.05):(0.95-1.05):(0.95-1.05):(0.1~0.3), mixing them evenly and then melting them at high temperature to obtain a cast alloy; rolling the cast alloy in multiple passes at room temperature, with a total rolling amount of not less than 50%; and annealing the rolled alloy to obtain a carbide-reinforced CoCrFeNi high-entropy alloy.

[0009] As a preferred embodiment of the above technical solution, the method for preparing carbide-reinforced CoCrFeNi high-entropy alloy provided by the present invention further includes some or all of the following technical features:

[0010] As an improvement to the above technical solution, the purity of the Co metal powder, Cr metal powder, Fe metal powder, Ni metal powder and TiC powder raw materials is greater than 99.9%, the particle size range of the powder is 0.05 to 200 μm, and the powder raw materials are mixed evenly.

[0011] As an improvement to the above technical solution, the high-temperature melting method is either electric arc melting or vacuum induction melting, with a melting temperature of 1500℃ ≤ melting temperature ≤ 2500℃.

[0012] As an improvement to the above technical solution, in the multi-pass rolling process, the rolling reduction in each pass is 5-10%, and the total rolling amount is not less than 50%. The multi-pass rolling process can be multi-pass cold rolling, multi-pass hot rolling, or a combination of cold rolling and hot rolling.

[0013] As an improvement to the above technical solution, the annealing process is carried out in a vacuum atmosphere or an argon atmosphere, the annealing temperature is 600-900℃, the holding time is 0.5-2h, and the cooling method is water cooling.

[0014] The carbide-reinforced CoCrFeNi high-entropy alloy described above exhibits excellent room-temperature strength and toughness, with a yield strength of 0.68–1.4 GPa, an ultimate tensile strength of 0.85–1.5 GPa, and an elongation of 1–22%.

[0015] Taking into account the strengthening effect of carbides and the advantages of rolling and annealing technologies, this invention designs and prepares a novel carbide-reinforced CoCrFeNi high-entropy alloy. The microstructure of the alloy is controlled by high-temperature melting, rolling and annealing, resulting in a high-entropy alloy material with excellent strength and toughness, which is expected to be used in aerospace structural components.

[0016] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0017] 1. This invention uses powder raw materials to prepare carbide-reinforced CoCrFeNi high-entropy alloys through high-temperature smelting technology. The powder is uniformly mixed, and the reaction during smelting is complete, effectively improving smelting efficiency. Furthermore, the alloy's microstructure is more uniform than when smelting bulk raw materials. Simultaneously, the smelting temperature is rationally controlled, falling between the melting and boiling points of pure metals, avoiding metal raw material loss and improving composition accuracy.

[0018] 2. This invention employs rolling and annealing methods to regulate the microstructure of as-cast alloys, thereby improving their strength and toughness. Rolling induces plastic deformation, significantly increasing dislocation density and generating a work-hardening effect, thus enhancing strength. Annealing causes the internal dislocations to recombine or disappear, restoring the material's toughness. During annealing at a specific temperature, partial recrystallization occurs in the alloy phase, with some grains forming fine recrystallized grains and others retaining high-density dislocations. The combined effects of dislocation strengthening and grain refinement enhance the alloy's strength and toughness. Simultaneously, during annealing, fine, dispersed second-phase carbide particles precipitate from the supersaturated alloy phase, further increasing the alloy's strength through dispersion strengthening.

[0019] 3. This invention prepares a novel carbide-reinforced CoCrFeNi high-entropy alloy system. The alloy consists of a highly ductile alloy phase, micron-sized carbide particles, and annealed micro / nano carbide particles, exhibiting a uniform microstructure and stable mechanical properties. The alloy possesses excellent room-temperature strength and toughness, with a yield strength of 0.68–1.4 GPa, an ultimate tensile strength of 0.85–1.5 GPa, and an elongation of 1–22%.

[0020] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of the present invention more apparent and understandable, the following detailed description is provided in conjunction with preferred embodiments. Attached Figure Description

[0021] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings of the embodiments will be briefly described below.

[0022] Figure 1 This is a schematic diagram of the rolling and heat treatment of the carbide-reinforced CoCrFeNi high-entropy alloy described in this invention;

[0023] Figure 2 Here is the XRD pattern of the carbide-reinforced CoCrFeNi high-entropy alloy prepared in Example 1 of this invention:

[0024] Figure 3 (a) is a microstructure diagram of the carbide-reinforced CoCrFeNi high-entropy alloy prepared in Example 1 of this invention:

[0025] Figure 3 (b) is a microstructure diagram of the carbide-reinforced CoCrFeNi high-entropy alloy prepared in Example 2 of the present invention:

[0026] Figure 3 (c) is a microstructure diagram of the carbide-reinforced CoCrFeNi high-entropy alloy prepared in Example 3 of the present invention:

[0027] Figure 3 (d) is a microstructure diagram of the carbide-reinforced CoCrFeNi high-entropy alloy prepared in Example 4 of the present invention;

[0028] Figure 4 This is a tensile stress-strain curve of the carbide-reinforced CoCrFeNi high-entropy alloy described in this invention. Detailed Implementation

[0029] The following detailed description of specific embodiments of the present invention is part of this specification. The principles of the present invention are illustrated through examples, and other aspects, features and advantages of the present invention will become apparent from this detailed description.

[0030] This invention adds hard TiC to a CoCrFeNi high-entropy alloy, and obtains a high-entropy alloy composed of an alloy matrix phase and carbides through high-temperature melting. Further, rolling and annealing treatments cause dynamic recrystallization of the matrix phase, precipitating fine and dispersed carbide particles. Through grain refinement strengthening and the second-phase strengthening effect of the two carbides, the overall strength and toughness of the alloy are improved, resulting in a carbide-reinforced CoCrFeNi high-entropy alloy with excellent room-temperature strength and toughness. The specific embodiments of this invention are described in detail below, which form part of this specification. Examples are used to illustrate the principles of the invention, and other aspects, features, and advantages of the invention will become apparent from this detailed description.

[0031] Example 1:

[0032] Preparation of CoCrFeNi(TiC) 0.1 High-entropy alloys. The specific steps are as follows:

[0033] (1) High-temperature smelting: 200g of pure metal powders of Co, Cr, Fe, Ni and TiC with a purity of 99.9% were weighed according to the molar ratio of Co / Cr / Fe / Ni / TiC of 0.95:1.05:1:1:0.1. The particle size of each pure metal powder was 5μm and the particle size of TiC powder was 200μm. The powder raw materials were manually mixed for 20min to obtain mixed powder. Then, it was pressed into blocks and smelted in a vacuum induction melting furnace at 1500℃ to obtain the cast alloy.

[0034] (2) Room temperature cold rolling: The cast alloy sample obtained in step 1 is subjected to cold rolling at room temperature, with a rolling reduction of 10% per pass and a total rolling amount of 75%.

[0035] (3) Annealing treatment: The cold-rolled alloy sample was placed in a tube furnace and annealed at 800℃ for 2 hours under an argon atmosphere. After that, it was taken out and water-quenched to room temperature to obtain CoCrFeNi(TiC). 0.1 High-entropy alloys.

[0036] Figure 2 Curve (a) represents the CoCrFeNi(TiC) prepared in Example 1. 0.1 The XRD pattern of the high-entropy alloy mainly shows the FCC high-entropy alloy phase and the (Ti,Cr,Co,Fe,Ni)C carbide phase. (Cr,Co,Fe,Ni,Ti) 23 The C6 carbide phase content was low and not shown in the XRD pattern. The obtained CoCrFeNi(TiC) phase... 0.1 High-entropy alloys consist of FCC high-entropy alloy phases, micron-sized (Ti,Cr,Co,Fe,Ni)C and (Cr,Co,Fe,Ni,Ti) phases. 23 C6 carbide particles, and micro / nano (Cr, Co, Fe, Ni, Ti) particles precipitated during annealing. 23 C6 carbide particle composition (e.g.) Figure 3 (as shown in (a)); the alloy has a yield strength of 0.68 GPa, an ultimate tensile strength of 0.85 GPa, and an elongation of 22%. Figure 4 (Curve a) represents the CoCrFeNi(TiC) prepared in Example 1. 0.1 Stress-strain curves of high-entropy alloys.

[0037] Example 2:

[0038] Preparation of CoCrFeNi(TiC) 0.2High-entropy alloys. The specific steps are as follows:

[0039] (1) High-temperature smelting: 200g of pure metal powders of Co, Cr, Fe, and Ni with a purity of 99.9% and TiC powder were weighed according to the molar ratio of Co / Cr / Fe / Ni / TiC of 1.05:0.95:0.95:1.05:0.2. The particle size of each pure metal powder was 44μm, and the particle size of TiC powder was 10μm. The powder raw materials were manually mixed for 15min to obtain mixed powder. Then, it was pressed into blocks and smelted in an electric arc melting furnace at 2200℃ to obtain the cast alloy.

[0040] (2) Two-step rolling: The as-cast alloy sample obtained in step 1 is rolled at 1150℃ with a rolling reduction of 6% per pass and a hot rolling reduction of 40%. Then it is held at 900℃ for 1 hour and cold rolled at room temperature with a rolling reduction of 10% per pass and a cold rolling reduction of 60%.

[0041] (3) Annealing treatment: The rolled alloy sample was placed in a tube furnace and annealed at 600℃ for 1 hour under an argon atmosphere. After that, it was taken out and water-quenched to room temperature to obtain CoCrFeNi(TiC). 0.2 High-entropy alloys.

[0042] Figure 2 Curve (b) represents the CoCrFeNi(TiC) prepared in Example 2. 0.2 The XRD pattern of the high-entropy alloy mainly shows the FCC high-entropy alloy phase and the (Ti,Cr,Co,Fe,Ni)C carbide phase. (Cr,Co,Fe,Ni,Ti) 23 The C6 carbide phase content was low and not shown in the XRD pattern. The obtained CoCrFeNi(TiC) phase... 0.2 The high-entropy alloy consists of FCC high-entropy alloy phase, micron-sized (Ti,Cr,Co,Fe,Ni)C carbides, and annealed (Ti,Cr,Co,Fe,Ni)C and (Cr,Co,Fe,Ni,Ti) precipitates. 23 C6 carbide particle composition (e.g.) Figure 3 (b) shows); the alloy has high strength, with a yield strength of 1.4 GPa, an ultimate tensile strength of 1.5 GPa, and a plastic strain of 1% (as shown in b); Figure 4 (Curve b) represents the CoCrFeNi(TiC) prepared in Example 2. 0.2 Stress-strain curves of high-entropy alloys.

[0043] Example 3:

[0044] Preparation of CoCrFeNi(TiC) 0.2 High-entropy alloys. The specific steps are as follows:

[0045] (1) High-temperature smelting: 200g of pure metal powders of Co, Cr, Fe, Ni and TiC with a purity of 99.9% were weighed according to the molar ratio of Co / Cr / Fe / Ni / TiC of 1:1:1.05:0.95:0.2. The particle size of each pure metal powder was 44μm and the particle size of TiC powder was 5μm. The powder raw materials were manually mixed for 10min to obtain mixed powder. Then, it was pressed into blocks and smelted in an electric arc melting furnace at 2000℃ to obtain a cast alloy.

[0046] (2) Room temperature cold rolling: The as-cast alloy sample obtained in step 1 is rolled at room temperature, with a rolling reduction of 10% per pass and a total rolling amount of 50%.

[0047] (3) Annealing treatment: The rolled alloy sample was placed in a tube furnace and annealed at 900℃ for 1 hour under an argon atmosphere. After that, it was taken out and water-quenched to room temperature to obtain CoCrFeNi(TiC). 0.2 High-entropy alloys.

[0048] Figure 2 Curve (c) represents the CoCrFeNi(TiC) prepared in Example 3. 0.2 The XRD pattern of the high-entropy alloy mainly shows the FCC high-entropy alloy phase and the (Ti,Cr,Co,Fe,Ni)C carbide phase. (Cr,Co,Fe,Ni,Ti) 23 The C6 carbide phase content was low and not shown in the XRD pattern. The obtained CoCrFeNi(TiC) phase... 0.2 High-entropy alloys consist of FCC high-entropy alloy phases, micron-sized (Ti,Cr,Co,Fe,Ni)C and (Cr,Co,Fe,Ni,Ti) phases. 23 C6 carbides, and micro / nano compounds (Cr, Co, Fe, Ni, Ti) precipitated during annealing. 23 C6 carbide particle composition (e.g.) Figure 3 (c) shown); the alloy has a yield strength of 0.75 GPa and a plastic strain of 13% ( Figure 4 (Curve c) represents the CoCrFeNi(TiC) prepared in Example 3. 0.2 Stress-strain curves of high-entropy alloys.

[0049] Example 4:

[0050] Preparation of CoCrFeNi(TiC) 0.3 High-entropy alloys. The specific steps are as follows:

[0051] (1) High-temperature smelting: 200g of pure metal powders of Co, Cr, Fe, Ni and TiC with a purity of 99.95% were weighed according to the molar ratio of Co / Cr / Fe / Ni / TiC of 1:1.05:1:0.95:0.3. The particle size of Fe was 0.05μm, the particle size of the other pure metal powders was 20μm, and the particle size of TiC powder was 44μm. The powder raw materials were manually mixed for 10min to obtain mixed powder. Then, it was pressed into blocks and smelted in an electric arc melting furnace at 2500℃ to obtain a cast alloy.

[0052] (2) High-temperature hot rolling: The as-cast alloy sample obtained in step 1 is hot rolled at 1150℃, with a rolling reduction of 5% per pass and a total rolling amount of 50%.

[0053] (3) Annealing treatment: The rolled alloy sample was placed in a tube furnace and annealed at 700℃ for 0.5h in a vacuum atmosphere. After that, it was taken out and water-quenched to room temperature to obtain CoCrFeNi(TiC). 0.3 High-entropy alloys.

[0054] Figure 2 Curve (d) represents the CoCrFeNi(TiC) prepared in Example 4. 0.3 The XRD pattern of the high-entropy alloy mainly shows the FCC high-entropy alloy phase and the (Ti,Cr,Co,Fe,Ni)C carbide phase. (Cr,Co,Fe,Ni,Ti) 23 The C6 carbide phase content was low and not shown in the XRD pattern. The obtained CoCrFeNi(TiC) phase... 0.3 High-entropy alloys consist of FCC high-entropy alloy phases, micron-sized (Ti,Cr,Co,Fe,Ni)C and (Cr,Co,Fe,Ni,Ti) phases. 23 C6 carbides, and (Ti,Cr,Co,Fe,Ni)C and (Cr,Co,Fe,Ni,Ti) precipitates from annealing. 23 C6 carbide particle composition (e.g.) Figure 3 (d) shows that the alloy has a yield strength of 0.70 GPa and an elongation of 11%. Figure 4 (Curve d) represents the CoCrFeNi(TiC) prepared in Example 3. 0.3 Stress-strain curves of high-entropy alloys.

[0055] The above description is merely a preferred embodiment of the present invention, and should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a carbide-reinforced CoCrFeNi high-entropy alloy, characterized in that, The process includes the following steps: Co metal powder, Cr metal powder, Fe metal powder, Ni metal powder and TiC powder are mixed evenly and then melted at high temperature to obtain a cast alloy; the cast alloy is rolled in multiple passes at room temperature, with a total rolling amount of not less than 50%; the rolled alloy is annealed to obtain a carbide-reinforced CoCrFeNi high-entropy alloy. The atomic ratio of the Co metal powder, Cr metal powder, Fe metal powder, Ni metal powder, and TiC powder is (0.95~1.05):(0.95~1.05):(0.95~1.05):(0.95~1.05):(0.1~0.3); the purity of the raw materials of the Co metal powder, Cr metal powder, Fe metal powder, Ni metal powder, and TiC powder is greater than 99.9%, and the particle size range of the powder is 0.05~200μm; The high-temperature melting method is either electric arc melting or vacuum induction melting, with a melting temperature of 1500℃ ≤ melting temperature ≤ 2500℃. The multi-pass rolling process has a rolling reduction of 5-10% per pass and a total rolling amount of not less than 50%; the multi-pass rolling process is a multi-pass cold rolling, a multi-pass hot rolling, or a mixed operation of cold rolling and hot rolling. The annealing process is carried out in a vacuum or argon atmosphere, with an annealing temperature of 600~900℃, a holding time of 0.5~2h, and a water cooling method.

2. A carbide-reinforced CoCrFeNi high-entropy alloy prepared by the method described in claim 1, characterized in that: The carbide-reinforced CoCrFeNi high-entropy alloy is composed of a face-centered cubic high-entropy alloy phase and a carbide phase; the high-entropy alloy phase is an FCC solid solution composed of Co, Cr, Fe, Ni and Ti elements; the carbide phase is (Cr, Co, Fe, Ni, Ti). 23 A mixture of C6 solid solution and (Ti, Cr, Co, Fe, Ni)C solid solution, wherein (Cr, Co, Fe, Ni, Ti) 23 The atomic ratio of Cr, Co, Fe, Ni, Ti, and C in the C6 solid solution is (50~53):(9~10):(8~10):(5~8):(1~2):(21~23), and the atomic ratio of Ti, Co, Fe, Ni, Cr, and C in the (Ti, Cr, Co, Fe, Ni)C solid solution is (20~22):(8~10):(8~10):(7~9):(8~10):(43~45). The microstructure of the high-entropy alloy consists of dendritic high-entropy alloy phases, interdendritic micron-sized carbide particles, and annealed micro-nano carbide particles, with good phase interface bonding. The yield strength of the carbide-reinforced CoCrFeNi high-entropy alloy is 0.68~1.4 GPa, the ultimate tensile strength is 0.85~1.5 GPa, and the elongation is 11~22%.

Citation Information

Patent Citations

  • Preparation method of metastable state high-entropy alloy with high-strength and high-plasticity heterogeneous grain structure

    CN115976349A

  • Durable high-entropy alloy punch and preparation method thereof

    CN117965992A