A processing method for low-roughness polished wafers based on heavily boron-doped material
By adjusting the stage parameters and optimizing the combination of polishing liquid cloth, the stability and effect problems of 1150-micron silicon wafers in the polishing process were solved, and a highly efficient surface polishing effect was achieved.
Patent Information
- Application Number
- CN202510143852.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-02-10
AI Technical Summary
Existing polishing processes are prone to causing 1150-micron silicon wafers to detach from the stage and break when processed, and the polishing effect is poor, failing to fully consider the characteristics of semiconductor materials.
By adjusting the stage rotation speed and vacuum adsorption pressure, and combining polishing liquids and polishing cloths with different particle sizes and solid contents, including SUBA600, SUBA800, CKE212S and silica polishing agents, the rough, medium and fine polishing processes are optimized.
It improves the stability and polishing effect of 1150-micron silicon wafers during the waxing process, ensuring that the silicon wafers do not break and significantly improving surface smoothness.
Smart Images

Figure CN119772666B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of silicon wafer processing technology, and more specifically, to a processing method for a heavily boron-doped, low-roughness polished wafer. Background Technology
[0002] In the field of semiconductor material manufacturing, surface polishing is a crucial process. Especially during the manufacturing of semiconductor devices, the surface roughness of semiconductor materials directly affects the performance and reliability of the devices. Therefore, surface polishing technology for semiconductor materials has always been a research hotspot in this field. In semiconductor device processing, surface polishing not only improves device performance and reliability but also increases device yield and reduces production costs. Thus, surface polishing technology for semiconductor materials is also one of the most important technologies in this field. In the field of surface polishing technology, polishing is an important means to achieve a smooth and flat surface on semiconductor materials. The polishing process includes multiple steps such as rough polishing, medium polishing, and fine polishing, each requiring the use of different polishing slurries and polishing cloths to achieve different polishing effects.
[0003] However, current polishing processes are prone to the following problems when processing 1150-micron silicon wafers:
[0004] 1. A 1150-micron silicon wafer is much heavier than a 725-micron silicon wafer. When the stage rotates the silicon wafer, the centrifugal force is also greater, making the silicon wafer more likely to detach from the stage and be thrown away, causing it to break.
[0005] 2. The characteristics of semiconductor materials were not fully considered when selecting polishing slurry and polishing cloth, resulting in poor polishing effect. Summary of the Invention
[0006] To address the aforementioned problems in the prior art, this invention provides a processing method for a heavily boron-doped low-roughness polished sheet.
[0007] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0008] A processing method for a heavily boron-doped low-roughness polished wafer, comprising:
[0009] The rotation speed of the stage and the vacuum adsorption pressure of the stage on the silicon wafer are set to adapt to the wax coating operation of 1150-micron silicon wafers.
[0010] When coarsely polishing the silicon wafer, a first polishing slurry with a particle size of 40-70 nanometers and a solid content of 13%-18% is selected, and two types of first polishing cloths, SUBA600 and SUBA800, are used in combination.
[0011] When polishing the silicon wafer, a second polishing slurry with a particle size of 30-70 nanometers and a solid content of 11%-15% is selected, and a second polishing cloth of model CKE212S is selected.
[0012] When polishing the silicon wafer, a third polishing slurry with a particle size of 20-40 nanometers and a solid content of 7-10% is used.
[0013] Preferably, the rotational speed of the stage is between 1700 RPM and 2500 RPM.
[0014] Preferably, the vacuum adsorption pressure of the stage on the silicon wafer is -85 kPa to -95 kPa.
[0015] Preferably, when the silicon wafer is subjected to intermediate polishing, the intermediate polishing pressure is set to 50-70 kPa.
[0016] Preferably, the intermediate polishing time for the silicon wafer is set to 15-20 minutes.
[0017] Preferably, when the silicon wafer is finely polished, the polishing pressure is set to 50-70 kPa.
[0018] Preferably, when the silicon wafer is finely polished, the polishing time is set to 15-20 minutes.
[0019] Preferably, when the silicon wafer is finely polished, the third polishing fluid is set to be discharged in a straight manner, and the flow rate is 1.5-2.5L / min.
[0020] Preferably, the first polishing liquid, the second polishing liquid, and the third polishing liquid all use silicon dioxide as the polishing agent.
[0021] The present invention has at least the following beneficial effects:
[0022] 1. In this application, the rotation speed of the stage and the vacuum adsorption pressure of the stage on the silicon wafer are adjusted for 1150-micron silicon wafers, so that the silicon wafer can have better stability when rotating with the stage, and improve the safety of wax coating operation on silicon wafers.
[0023] 2. This application fully considers the material characteristics of 1150-micron silicon wafers and selects appropriate polishing fluids and polishing cloths when performing rough polishing, medium polishing and fine polishing of silicon wafers, so as to achieve better polishing effect. Attached Figure Description
[0024] Figure 1 A flowchart of a processing method based on a heavily boron-doped low-roughness polished sheet is shown in some embodiments of this application. Detailed Implementation
[0025] To further understand the content of this invention, a detailed description of the invention will be provided in conjunction with the accompanying drawings and embodiments. It should be understood that the embodiments are merely illustrative and not limiting of the invention.
[0026] like Figure 1 As shown, this embodiment provides a processing method for a heavily boron-doped low-roughness polished wafer. This processing method is suitable for processing 1150-micron silicon wafers. On the one hand, it can improve the stability and safety of the silicon wafer during the waxing process, and on the other hand, it can improve the polishing effect of the silicon wafer.
[0027] The processing method includes:
[0028] Step S100: Set the rotation speed of the stage and the vacuum adsorption pressure of the stage on the silicon wafer to adapt to the wax coating operation of 1150-micron silicon wafers.
[0029] Understandably, 1150-micron silicon wafers are heavier than conventional 725-micron silicon wafers. This means that after the stage vacuum adsorbs the silicon wafer, the stage rotates the wafer, resulting in greater centrifugal force. If conventional processes are used, the silicon wafer is prone to detaching from the stage and being flung away, potentially causing it to break. Therefore, in this embodiment, the rotation speed of the stage and the vacuum adsorption pressure of the stage on the 1150-micron silicon wafer are adjusted to ensure better stability when the silicon wafer rotates with the stage, thus improving the safety of the wax coating operation.
[0030] Step S200: When coarsely polishing the silicon wafer, a first polishing slurry with a particle size of 40-70 nanometers and a solid content of 13%-18% is selected, and two types of first polishing cloths, SUBA600 and SUBA800, are used together.
[0031] It is understandable that by using a first polishing slurry with a particle size of 40-70 nanometers and a solid content of 13%-18% to perform rough polishing on silicon wafers, and by using two types of first polishing cloths, namely SUBA600 and SUBA800, to perform rough polishing on silicon wafers, the surface roughness of silicon wafers can reach 0.6nm, resulting in a better surface polishing effect on silicon wafers.
[0032] Step S300: When performing intermediate polishing on the silicon wafer, a second polishing slurry with a particle size of 30-70 nanometers and a solid content of 11%-15% is selected, and a second polishing cloth of model CKE212S is selected.
[0033] It should be noted that the second polishing cloth, model CKE212S, has a pore size of 80±23 micrometers, which allows the silicon wafer to be further polished after rough polishing by passing through the second polishing cloth.
[0034] It is understandable that by using a second polishing slurry with a particle size of 30-70 nanometers and a solid content of 11%-15% to perform intermediate polishing on silicon wafers, and by using a second polishing cloth of model CKE212S to perform intermediate polishing on silicon wafers, the surface roughness of silicon wafers can be reduced to 0.3nm, resulting in a better surface polishing effect on silicon wafers.
[0035] Step S400: When performing fine polishing on the silicon wafer, a third polishing slurry with a particle size of 20-40 nanometers and a solid content of 7-10% is used.
[0036] It is understandable that by using a third polishing slurry with a particle size of 20-40 nanometers and a solid content of 7-10% to perform fine polishing on silicon wafers, the surface roughness of the silicon wafers can be reduced to below 0.17nm, resulting in a better surface polishing effect.
[0037] In some embodiments, in step S100, after the stage vacuum adsorbs the silicon wafer, the stage rotation speed is set to 1700 RPM-2500 RPM, so that the silicon wafer rotates with the stage at a speed of 1700 RPM-2500 RPM. It can be understood that this embodiment, by setting the stage rotation speed, allows the stage rotation speed to be better adapted to the wax coating operation of 1150-micron silicon wafers, and can better ensure the stability of the silicon wafer's position on the stage. On the one hand, it enables the wax coating operation of the silicon wafer, and on the other hand, it prevents the silicon wafer from being thrown away by the stage.
[0038] In some embodiments, in step S100, the vacuum adsorption pressure of the stage on the silicon wafer is set to -85 kPa to -95 kPa. It is understood that by setting the vacuum adsorption pressure of the stage on the silicon wafer in this embodiment, the stage can maintain a better adsorption force on the silicon wafer during the rotation process, thereby improving the stability of the silicon wafer on the stage and preventing the silicon wafer from being thrown off by the stage.
[0039] In some embodiments, in step S300, when performing intermediate polishing on the silicon wafer, the intermediate polishing pressure is set to 50-70 kPa. This setting ensures that the silicon wafer undergoes sufficient intermediate polishing, enabling the surface roughness of the silicon wafer to reach 0.3 nm, thereby improving the polishing effect of the silicon wafer.
[0040] In some embodiments, in step S300, the intermediate polishing time for the silicon wafer is set to 15-20 minutes. This setting ensures sufficient time for the intermediate polishing process, allowing the surface roughness of the silicon wafer to reach 0.3 nm, thereby improving the polishing effect.
[0041] In some embodiments, during step S400, the polishing pressure is set to 50-70 kPa when performing fine polishing on the silicon wafer. This setting ensures sufficient fine polishing of the silicon wafer, enabling the surface roughness of the silicon wafer to reach below 0.17 nm, thereby improving the polishing effect of the silicon wafer.
[0042] In some embodiments, in step S400, the fine polishing time for the silicon wafer is set to 15-20 minutes. This setting ensures sufficient time for fine polishing, allowing the surface roughness of the silicon wafer to reach below 0.17 nm, thereby improving the polishing effect.
[0043] In some embodiments, in step S400, when performing fine polishing on the silicon wafer, the third polishing fluid is selected in a direct discharge manner, and the direct discharge flow rate is 1.5-2.5L / min.
[0044] In some embodiments, the first polishing slurry, the second polishing slurry, and the third polishing slurry used in the rough polishing, medium polishing, and fine polishing processes of silicon wafers all use silicon dioxide as a polishing agent.
[0045] More specifically, since the first polishing slurry uses silica as the polishing agent, the silica particle size in the first polishing slurry is 40-70 nanometers, and the solid content of silica in the first polishing slurry is 13%-18%. Since the second polishing slurry uses silica as the polishing agent, the silica particle size in the second polishing slurry is 30-70 nanometers, and the solid content of silica in the second polishing slurry is 11%-15%. Since the third polishing slurry uses silica as the polishing agent, the silica particle size in the third polishing slurry is 20-40 nanometers, and the solid content of silica in the third polishing slurry is 7-10%.
[0046] In summary, the above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be covered by the present invention.
Claims
1. A processing method for a heavily boron-doped low-roughness polished sheet, characterized in that: include, The rotation speed of the stage and the vacuum adsorption pressure of the stage on the silicon wafer are set to adapt to the wax coating operation of 1150-micron silicon wafers. When coarsely polishing the silicon wafer, a first polishing slurry with a particle size of 40-70 nanometers and a solid content of 13%-18% is selected, and two types of first polishing cloths, SUBA600 and SUBA800, are used in combination. When polishing the silicon wafer, a second polishing slurry with a particle size of 30-70 nanometers and a solid content of 11%-15% is selected, and a second polishing cloth of model CKE212S is selected. When polishing the silicon wafer, a third polishing slurry with a particle size of 20-40 nanometers and a solid content of 7-10% is used. The vacuum adsorption pressure of the stage on the silicon wafer is -85 kPa to -95 kPa. When the silicon wafer is finely polished, the third polishing fluid is set to be discharged directly, and the flow rate is 1.5-2.5L / min; The first polishing liquid, the second polishing liquid, and the third polishing liquid all use silicon dioxide as a polishing agent.
2. The processing method according to claim 1, characterized in that: The stage rotates at a speed of 1700 RPM to 2500 RPM.
3. The processing method according to claim 1, characterized in that: When the silicon wafer is subjected to intermediate polishing, the intermediate polishing pressure is set at 50-70 kPa.
4. The processing method according to claim 1, characterized in that: When the silicon wafer is subjected to intermediate polishing, the intermediate polishing time is set to 15-20 minutes.
5. The processing method according to claim 1, characterized in that: When the silicon wafer is finely polished, the polishing pressure is set at 50-70 kPa.
6. The processing method according to claim 1, characterized in that: When the silicon wafer is finely polished, the polishing time is set to 15-20 minutes.
Citation Information
Patent Citations
Method for improving flatness of polished silicon wafer
CN111230605A
Wax surface mounting process for high-quality geometric parameter polished wafer
CN114310653A