An anti-glare PMMA polarizing film
By applying an anti-glare coating to a PMMA optical film substrate and performing UV curing, combined with Corona treatment and pressure-sensitive adhesive, the problems of insufficient anti-glare performance and coating adhesion of polarizers are solved, achieving efficient and stable polarizer production.
Patent Information
- Application Number
- CN202510083039.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-01-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-01-20
AI Technical Summary
Existing polarizers have poor anti-glare performance, poor coating adhesion and insufficient wear resistance, and traditional processes suffer from uneven coating, easy peeling and poor optical performance.
It uses PMMA optical film substrate with an anti-glare coating on the surface. The coating consists of acrylate prepolymer, acrylate monomer, photoinitiator, surfactant and silicon particles. It forms an adhesive layer through UV curing process and is treated with Corona before coating to enhance adhesion. UV adhesive is used instead of water-based thermosetting adhesive and combined with pressure-sensitive adhesive protective film.
It improves the anti-glare effect of polarizers, enhances the uniformity and adhesion of coatings, reduces the risk of dimensional changes and peeling, improves wear resistance and stability, and shortens the production cycle.
Smart Images

Figure CN119937078B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an anti-glare PMMA type polarizer, belonging to the field of polarizer technology. Background Technology
[0002] Polarizing films are becoming increasingly widely used, playing an important role in homes, offices, and outdoor advertising. As product development demands, the development of high contrast, wide viewing angle, thinness, large size, high precision, and diversified additional functions is necessary to meet human needs.
[0003] Most monitors are used in environments with external light sources, which can cause glare due to reflection. To enhance the visual experience, an anti-glare film is used on the outermost layer of the monitor to reduce the negative effects of specular reflection on the human eye and to reduce reflected light caused by external ambient light.
[0004] Large-size LCD displays are mostly used in outdoor commercial displays, requiring that polarizers not be affected by moisture in hot and humid environments, which would reduce polarization ability, affect the durability of the polarizer, and cause problems such as light leakage, yellowing, and uneven color. Therefore, ultra-large-size polarizers have extremely stringent requirements for weather resistance and water resistance. Traditional coating processes have problems such as uneven coating, easy peeling, and poor optical performance, which cannot achieve the technical purpose well. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art, namely the poor anti-glare performance, poor coating adhesion, and insufficient wear resistance in the preparation of existing polarizers.
[0006] To solve the above-mentioned technical problems, the present invention is implemented using the following technical solution: An anti-glare PMMA polarizer is provided, comprising: a PMMA optical film substrate; the surface of the substrate is provided with an anti-glare coating; The anti-glare coating comprises acrylate prepolymer, acrylate monomer, photoinitiator, surfactant, and silicon particles; The acrylate prepolymer and acrylate monomer are mixed in a solvent, then a photoinitiator and a surfactant are added to form a first mixture, and finally silicon particles are added to form a coating composition. The coating composition is provided with a pretreatment process before surface coating, and a multi-stage drying process after coating, followed by a UV curing process; after the UV curing process, a protective film is applied, and a pressure-sensitive adhesive is provided on the outside of the protective film. The PMMA has two layers, which are respectively attached to both sides of the PVA film.
[0007] Furthermore, the solvent includes ketones, esters, and benzenes.
[0008] Furthermore, the photoinitiator is a free radical photoinitiator, which polymerizes with acrylate monomers under UV irradiation.
[0009] Furthermore, the pretreatment process includes oven preheating and plasma cleaning of PMMA; The plasma cleaning is performed on both PMMA films before UV curing.
[0010] Furthermore, the UV curing process includes: The PVA layer and the PMMA layer are bonded together using a UV-curable adhesive, which cures under ultraviolet light to form an adhesive layer.
[0011] Furthermore, the UV curing process includes at least three curing units.
[0012] Furthermore, the protective film is adhered to the surface of the coating, and a pressure-sensitive adhesive is provided on the outer side of the protective film.
[0013] Furthermore, the adhesion of the pressure-sensitive adhesive is within 300gf / 25mm.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: 1. This invention uses an anti-glare optical film as a protective layer on the PVA film, and incorporates silicon particles in the anti-glare composition, resulting in a large surface area. These particles are uniformly dispersed in the coating liquid to achieve diffuse reflection, achieving a haze of over 25%. Simultaneously, a novel adhesive for the PVA and PMMA layers of the polarizer is developed: a UV adhesive replaces the water-based thermosetting adhesive. By adjusting process parameters, the drying speed of the polarizer is moderated, reducing inter-component thermal variations that could lead to dimensional differences and thus lowering the risk of peeling delamination due to weak adhesion. Attached Figure Description
[0015] Figure 1 The diagram shown illustrates the preparation process of the anti-glare coating of this invention. Figure 2 The diagram shown is a flow chart of the surface coating production process of this invention. Figure 3 The diagram shown is a PMMA bonding diagram of the present invention. Detailed Implementation
[0016] The present invention will be further described below with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and should not be used to limit the scope of protection of the present invention.
[0017] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art will understand the specific meaning of the above terms in this invention based on the specific circumstances. Example 1:
[0018] An anti-glare PMMA polarizer is provided, comprising: a PMMA optical film substrate; the surface of the substrate is provided with an anti-glare coating; The anti-glare coating comprises acrylate prepolymer, acrylate monomer, photoinitiator, surfactant, and silicon particles; The acrylate prepolymer and acrylate monomer are mixed in a solvent, then a photoinitiator and a surfactant are added to form a first mixture, and finally silicon particles are added to form a coating composition. The coating composition is provided with a pretreatment process before surface coating, and with multiple drying processes after coating, followed by a UV curing process.
[0019] The main components of the anti-glare coating include acrylate prepolymer, acrylate monomer, photoinitiator, surfactant, and silica particles. The acrylate prepolymer and acrylate monomer are the base materials of the coating, capable of polymerization under ultraviolet light to form a rigid coating structure.
[0020] Photoinitiators are used to initiate polymerization reactions under ultraviolet irradiation, enabling the coating to cure in a short time; surfactants reduce the surface tension of the coating liquid, improve its fluidity and wettability, and ensure that the coating is evenly covered on the substrate surface; silicon particles, as additives to enhance the anti-glare effect of the coating, provide a certain degree of haze, giving the coating a strong ability to scatter light, and further improving the anti-glare effect.
[0021] like Figure 1 As shown, the preparation of the coating composition first involves mixing acrylate prepolymer and acrylate monomer in a solvent, including ketones, esters, and benzenes, which effectively reduce the viscosity of the coating solution, allowing the coating to be uniformly applied to the PMMA substrate surface. After mixing, a photoinitiator and surfactant are added to the solution, which helps to initiate the polymerization reaction during UV curing and improves the coating's flowability and adhesion. Finally, silica particles are added, which help improve the coating's haze, anti-glare effect, and enhance its abrasion resistance and scratch resistance.
[0022] like Figure 2As shown, the PMMA optical film undergoes pretreatment before coating. In this actual production, Corona treatment is selected. This involves using a high voltage to generate an electric field between two electrodes, forming high-energy electrons and oxygen molecules near the substrate surface, thereby activating the substrate surface. During this process, the film surface is exposed to high-energy ions, free radicals, and ozone gases. These substances react with the molecules on the film surface, breaking down molecular chains and creating an active surface containing polar groups. This ensures the uniformity and good adhesion of the coating.
[0023] Simultaneously, the PVA film is preheated, and then the Corona-treated PMMA is bonded to both sides of the PVA film. The surface of the PMMA film has been coated with a UV-curable adhesive. The PMMA film and PVA film are then bonded together and cured under UV light. Finally, AG particle coating is applied, and similarly, UV curing is required after coating. The coating undergoes multiple drying processes to remove excess solvent, ensuring the stability and uniformity of the coating during further processing.
[0024] During the UV curing process, the UV-curable adhesive is cured under ultraviolet light to form an adhesive layer. The coating is cured using the energy of ultraviolet light, ensuring its hardness and durability; and the UV curing process includes at least three curing units.
[0025] By using UV adhesives instead of water-based thermosetting adhesives, the photoinitiator in the UV-cured material absorbs ultraviolet light under UV irradiation and generates active free radicals or cations, initiating monomer polymerization and cross-linking chemical reactions, causing the adhesive to transform from a liquid to a solid state within seconds. The photoinitiator (PI) changes from a ground state to an excited state under UV irradiation, and then decomposes into free radicals. The free radicals combine with monomers and carry out chain growth, causing carbon-carbon double bonds to polymerize. This process is accompanied by the transfer and termination of free radicals on the growing chain, reducing the curing time from 3 minutes for water-based thermosetting adhesives to just a few seconds, which can greatly simplify the original equipment such as ovens.
[0026] The protective film is adhered to the surface of the coating, and a pressure-sensitive adhesive is provided on the outer side of the protective film. The protective film not only protects the coating from damage but also keeps the coating clean during the production, transportation, and use of the polarizer. The pressure-sensitive adhesive on the outer side of the protective film provides sufficient adhesion to ensure the film layer firmly adheres to the surface without the need for additional heating or pressure.
[0027] The pressure-sensitive adhesive has an adhesion strength of less than 300 gf / 25 mm, ensuring strong adhesion of the protective film while facilitating subsequent removal or replacement. The low adhesion strength prevents damage to the coating or substrate during film removal, ensuring easy and non-destructive removal and providing greater processing flexibility.
[0028] like Figure 3 As shown, because pressure-sensitive adhesive (PSA) has high adhesive strength, it can easily lead to rework difficulties during panel reworking, and even the possibility of polarizer breakage. Increasing the gel fraction of PSA reduces its adhesive strength. Simultaneously, as the PSA thickness decreases, the storage modulus of the PSA layer tends to increase when external stress is applied at high speed, effectively suppressing the formation of nano-slits. A higher storage modulus means a harder PSA adhesive, lower chain segment mobility, and reduced adhesive hysteresis; during peeling, energy is dissipated through molecular chain movement, resulting in lower peeling force and improving the difficulty of peeling during rework.
[0029] Traditional methods for preparing anti-glare polarizers typically involve first coating an anti-glare coating onto a PMMA substrate, followed by UV curing to obtain an anti-glare PMMA optical film (AG-PMMA). Then, the AG-PMMA (upper T), PMMA compensation film (lower T), and PVA are laminated together, followed by another curing. This traditional process usually requires the AG-PMMA film to be manufactured on a separate production line, then wound back and transported to the polarizer production line to be laminated with the PMMA compensation film and PVA. In contrast, this embodiment first laminates a general-purpose PMMA and PMMA compensation film onto PVA, then directly coats the surface of the general-purpose PMMA with an anti-glare coating, completing the anti-glare polarizer process in one step. This significantly shortens the manufacturing cycle of anti-glare polarizers and improves polarizer manufacturing efficiency. Furthermore, in this embodiment, the PMMA film surface is treated with a corona process before coating, enhancing the adhesion between the PMMA and PVA films and ensuring a strong bond between the substrate surface and the PVA film before applying the anti-glare coating. The corona treatment between the PMMA and PVA films improves the adhesion between the two layers, reducing the risk of coating peeling and ensuring long-term product stability. Simultaneously, the UV curing process not only guarantees the coating's hardness and anti-glare effect but also effectively enhances interlayer adhesion, resulting in a final product with higher wear resistance and stability during use. Example 2:
[0030] like Figure 2 As shown, all components must be thoroughly mixed before addition. The solvent, acrylate prepolymer, and acrylate monomers should be mixed in a stirrer to ensure complete dissolution and prevent polymer precipitation.
[0031] When preparing the coating solution, first add ketone, ester, or benzene solvents to the reaction vessel and stir slowly to reduce the viscosity of the solvent, achieving ideal coatability. Then add the photoinitiator and surfactant to the solvent mixture, ensuring the photoinitiator is completely dissolved and the surfactant is evenly distributed in the coating solution to ensure uniform coating and good adhesion.
[0032] Finally, add the pre-prepared silicon particles and disperse them efficiently to ensure uniform distribution of the particles in the coating solution. Ultrasonic or high-shear stirring can be used to aid dispersion and prevent particle sedimentation or agglomeration.
[0033] During the surface coating process, the PVA film serves as the intermediate layer, and PMMA serves as the cover layers on both sides. The PMMA films are sent to the Corona treatment equipment for surface activation. The Corona treatment generates corona discharge between the electrodes through high voltage. The high-energy ions, free radicals, and ozone generated by the corona discharge react with the molecules on the surface of the PMMA film, breaking the molecular chains and introducing polar groups, thereby significantly increasing the surface energy of the PMMA film and enhancing its adhesion to the PVA film.
[0034] Typically, each PMMA film is processed in the Corona device for 5-10 seconds, depending on the film thickness, surface quality, and required level of activity. A UV-curable adhesive is applied to the bonding surfaces of the PMMA and PVA films. The Corona-treated PMMA film is then bonded to both sides of the PVA film. Because both sides of the PMMA film are Corona-treated, they adhere better to the surface of the PVA film.
[0035] UV adhesives have good optical transparency and hardness, and can effectively enhance the adhesion between film layers, ensuring the stability of the entire multilayer structure.
[0036] The film, coated with UV adhesive and laminated, is exposed to UV light, followed by the coating of AG particles, and then enters a UV curing device. The UV curing process includes at least three UV curing units, namely UV-1, UV-2, and UV-3. The exposure time and light source intensity of each unit are adjusted according to the film thickness, coating type, and desired curing effect. In each curing unit, ultraviolet irradiation triggers the photoinitiator in the adhesive to react, forming a strong adhesive layer. The curing time is preferably 5-20 seconds per unit.
[0037] After curing, the coating should be cooled at room temperature to ensure its stability. If further enhancement of coating adhesion or abrasion resistance is required, plasma cleaning or surface treatment can be performed; subsequently, automated optical inspection (AOI) should be used to check the coating's uniformity, thickness, and surface defects.
[0038] Finally, the coated substrate is wound up and then wound up by a fabric storage machine for subsequent packaging, transportation, or direct application.
[0039] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. An anti-glare PMMA polarizing film, characterized in that, include: PMMA optical film substrate; The substrate surface is provided with an anti-glare coating; The anti-glare coating comprises acrylate prepolymer, acrylate monomer, photoinitiator, surfactant, and silicon particles; The acrylate prepolymer and acrylate monomer are mixed in a solvent, then a photoinitiator and a surfactant are added to form a first mixture, and finally silicon particles are added to form a coating composition. The PMMA has two layers and is attached to both sides of the PVA film respectively; Before coating, the PMMA optical film is pretreated by Corona treatment; at the same time, the PVA film is preheated. After preheating, the Corona-treated PMMA is bonded to both sides of the PVA film. The surface of the PMMA film has been coated with a UV-curable adhesive and then cured by UV light. The UV curing process includes at least three curing devices. After UV curing, AG particles are coated. After coating, there are multiple drying processes, followed by a UV curing process, which includes at least three curing devices. After the UV curing process, a protective film is applied, and a pressure-sensitive adhesive is placed on the outside of the protective film.
2. The anti-glare PMMA polarizer according to claim 1, characterized in that, The solvents include ketones, esters, and benzenes.
3. The anti-glare PMMA polarizer according to claim 1, characterized in that, The photoinitiator is a free radical photoinitiator, which polymerizes with acrylate monomers under UV irradiation.
4. The anti-glare PMMA polarizer according to claim 1, characterized in that, The protective film is adhered to the surface of the coating, and a pressure-sensitive adhesive is provided on the outer side of the protective film.
5. The anti-glare PMMA polarizer according to claim 4, characterized in that, The adhesion of the pressure-sensitive adhesive is within 300gf / 25mm.
Citation Information
Patent Citations
Anti-dazzle liquid, anti-dazzle film, preparation method of anti-dazzle film and polaroid
CN115491119A
Ultraviolet curing adhesive, polarizing plate and preparation method
CN115505358A