A method for improving the service performance of the softened zone of flash welded joints in rails
By performing secondary heating and accelerated cooling on the flash welded joints of rails, and optimizing the heating and cooling processes, the problem of insufficient hardness and toughness in the softened zone of the rail welded joints was solved, significantly improving the overall service performance of the welded joints.
Patent Information
- Application Number
- CN202510290230.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-03-12
AI Technical Summary
The softened zone of rail welded joints has low hardness and toughness, which leads to rapid wear of the welded joints under high-volume and heavy-haul railway conditions and a shorter service life than the base material. Existing post-weld heat treatment processes are still insufficient in reducing the width of the softened zone and improving service performance.
The flash welded joints of rails that have cooled to a certain temperature after welding are reheated by combining a single heating device and an auxiliary heating device, followed by local accelerated cooling. The heating and cooling processes are optimized to refine the grains and improve the microstructure.
It significantly improves the hardness and toughness of the softened zone of the welded joint, reduces the collapse phenomenon, and makes the performance of the welded joint close to that of the base material, extending its service life and greatly reducing the width of the softened zone.
Smart Images

Figure CN119979859B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rail welding, and more specifically, to a method for improving the service performance of the softened zone of a flash welded joint in rails. Background Technology
[0002] In recent years, with the rapid development of railway transportation, especially the continuous increase in the freight volume, axle load, and maximum single-train load of heavy-haul railways, the wear and damage problems of rails and their welded joints have become increasingly serious. Whether aluminothermic welding or flash welding, under the heat-affected zone of welding, the rail surface hardness of the welded joint, especially in the softened zone, is lower than that of the base material, resulting in a reduction in its tensile strength, hardness, fatigue strength, and other mechanical properties. Under high-volume conditions, the wear in the softened zone of the welded joint is even faster, and the collapse phenomenon is very severe, leading to a shorter joint life than that of the rail base material.
[0003] Studies have shown that low slump in the softened zone of welded joints, impact wear, and fatigue wear caused by rolling contact are important causes of welded joint damage. The softened zone of a flash welded rail joint refers to the area where the hardness of the welded joint is significantly lower than that of the base material. The metal in this area does not undergo austenitic transformation during heating but is instead in the annealing range of heat treatment, hence it is also called the annealing zone or spheroidizing annealing zone. Since rail welding mainly involves localized heating of the rail ends, a transition zone always exists between the heated part and the unheated base material. The area with lower hardness in this transition zone is the softened zone. The presence of the softened zone results in poor tensile and impact properties of the welded joint, making it a weak point in the rail joint.
[0004] Currently, rail welding mainly employs two methods: flash welding and aluminothermic welding. The overall mechanical properties of aluminothermic welded joints are significantly lower than those of the base material, with weld strength and rail service life typically only reaching one-third to three-quarters of the base material's strength. In contrast, flash welding of rails is performed using mobile flash welding machines, offering a high degree of automation, stable process, and excellent weld quality. The welded joint has a dense forged structure, and its mechanical properties are close to those of the rail base material, making it the most practical, precise, and high-quality method for rail welding. However, even with flash welding, the performance of the softened zone in the welded joint still cannot meet the requirements of high-capacity and heavy-haul railways.
[0005] To address the aforementioned issues, existing technologies employ post-weld heat treatment processes, which improve the performance of welded joints by reheating for austenitization and controlling cooling. For example, using medium-frequency induction heating and jet cooling can enhance the surface hardness and toughness of the welded joint. However, existing technologies still have shortcomings, particularly in reducing the width of the softened zone and improving its overall service performance, which requires further optimization. Therefore, existing technologies still need improvement. Summary of the Invention
[0006] In view of this, the present invention aims to provide a method for improving the service performance of the softened zone of a rail flash weld joint. By optimizing the heating and cooling process, the width of the softened zone of the joint is significantly reduced, and the overall service performance of the softened zone is significantly improved. This method can at least solve the technical problem of the low service performance of the softened zone of existing rail flash weld joints.
[0007] The present invention proposes a method for improving the service performance of the softened zone of flash welded joints in rails, comprising: The flash welded joints of the rails, after cooling to a certain temperature following welding, undergo secondary heating. The heating process includes a normal heating stage and a special heating stage. In the normal heating stage, a single heating device is used to heat the entire cross-section of the flash welded joint. In the special heating stage, a single heating device is used to heat the entire cross-section of the flash welded joint, while an auxiliary heating device is used to supplement the heating of the rail heads at both ends of the area covered by the single heating device. After the rail flash welded joint is heated to the preset temperature, the single heating device and the auxiliary heating device are immediately removed, and a cooling device is used to accelerate the cooling of the local area on both sides of the fusion line of the rail flash welded joint that has been heated to the preset temperature.
[0008] In some embodiments, the starting temperature of the entire heating process is <300°C, and the ending temperature of the entire heating process is 900°C to 1100°C. The preset temperature is the ending temperature of the entire heating process.
[0009] In some embodiments, the starting temperature of the normal heating stage is <300°C, the ending temperature of the normal heating stage is 500°C to 600°C, and the duration is ≤100s.
[0010] In some embodiments, during a special heating phase, the temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating phase is ≤20°C, until the end temperature of the entire heating process is reached and the process terminates.
[0011] In some embodiments, a single heating device employs an induction coil with a profile mimicking that of a steel rail. The distance between the induction coil and the rail surface is 5mm to 50mm, and the heating area covers the entire weld joint area. The length of the heating device along the rail extension direction is 60mm to 150mm. During the normal heating stage, the single heating device controls the temperature rise rate of the entire cross-section of the flash welded joint of the rail to be 1.0℃ / s to 20.0℃ / s.
[0012] In some embodiments, during a special heating stage, the area assisted in heating by the auxiliary heating device is located at both ends of the weld joint area, and is the rail head working area including the rail top surface, rail head fillet, and rail head side surface.
[0013] In some embodiments, the length of the auxiliary heating device along the extension direction of the rail is 20mm to 30mm, the center line of the area covered by the auxiliary heating device coincides with the edge covered by the single heating device, and the duration of auxiliary heating is <40s.
[0014] In some embodiments, the average cooling rate of accelerated cooling is 5°C / s to 35°C / s, and the termination temperature of accelerated cooling is 200°C to 400°C.
[0015] In some embodiments, the local area cooled by the cooling device includes a transition area between the heated area and the unheated joint base material area during the heating process, and the temperature of the local area is 400°C to 600°C when heated to the end temperature of the entire heating process.
[0016] In some embodiments, the cooling device is a contact-type heat-conducting device that mimics the profile of a steel rail. The cooling device has a hollow structure, and heat exchange is carried out inside through a cooling medium. The contact surface between the cooling device and the steel rail is coupled with a flexible heat-conducting material.
[0017] In some embodiments, the cooling device includes a first cooling section that contacts the top surface of the rail head and a second cooling section that contacts the rounded corners and side surfaces of the rail head. The thickness of the first cooling section and the second cooling section is 15 mm to 30 mm, and the length along the rail extension direction is 20 mm to 40 mm.
[0018] The beneficial effects of this invention are as follows: By subjecting the flash welded rail joint to secondary heating and accelerated cooling after welding and cooling to a certain temperature, this invention significantly improves the hardness and toughness of the softened zone of the weld joint, reduces the low-slump phenomenon of the weld joint, and enhances the service performance of the softened zone of the flash welded rail joint. The optimized heat treatment process can effectively improve the microstructure of the weld joint, reduce the occurrence of unfavorable structures such as martensite, thereby improving the overall performance of the weld joint and extending its service life. Furthermore, the width of the softened zone on one side of the flash welded rail joint treated by the above method can be controlled to less than 5mm, a significant reduction compared to traditional processes. The average hardness of the softened zone is increased by more than 95% compared to the post-weld air-cooled joint, approaching the hardness level of the base material. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other embodiments can be obtained based on these drawings without creative effort.
[0020] Figure 1 This is a front view schematic diagram of the heating and cooling area of a rail flash welding head according to an embodiment of the present invention; Figure 2 This is a left-side view of the heating and cooling area of a rail flash welding head according to an embodiment of the present invention. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0022] It should be noted that all uses of "first" and "second" in the embodiments of the present invention are for the purpose of distinguishing two entities or parameters with the same name but different names. It is clear that "first" and "second" are only for the convenience of expression and should not be construed as limiting the embodiments of the present invention. Subsequent embodiments will not explain this in detail.
[0023] The present invention provides a method for improving the service performance of the softened zone of a flash welded joint in rails, comprising: The flash-welded rail joints, cooled to a certain temperature (e.g., below 300°C) after welding, undergo secondary heating. The heating process includes a standard heating stage and a special heating stage. In the standard heating stage, a single heating device heats the entire cross-section of the flash-welded rail joint. In the special heating stage, the single heating device continues to heat the entire cross-section of the flash-welded rail joint, while an auxiliary heating device is used to supplement the heating of the rail heads at both ends of the area covered by the single heating device. This further optimizes the heating effect, makes the heating more precise, and avoids localized overheating or underheating. Preferably, the auxiliary heating device mainly uses non-contact heating, such as flame or laser.
[0024] After the rail flash welded joint is heated to the preset temperature, the single heating device and the auxiliary heating device are immediately removed, and a cooling device is used to accelerate the cooling of the local area on both sides of the fusion line of the rail flash welded joint heated to the preset temperature, so as to effectively refine the grain size of the welded joint and improve the microstructure.
[0025] In this application, the flash welded joint of the rail includes a fusion line, a heat-affected zone (HAZ), and a base metal region. The flash welded joint is centered on the fusion line, which is the area formed by the resolidification of the material at both ends of the rail during welding, ensuring the physical connection between the two ends. The width of the fusion line is 0.5 mm to 2.0 mm. The HAZ is the area affected by heat during welding but not melted, located on both sides of the fusion line, with a width of 5.0 mm to 30.0 mm on each side. The base metal region is the area not affected by heat during welding, located on the side of the HAZ furthest from the fusion line, with a width of 5.0 mm to 20.0 mm on each side.
[0026] In this application, the microstructure of the rail is pearlitic. In the chemical composition of the rail, the mass fraction of C is 0.35% to 1.20%, the mass fraction of Si is 0.10% to 1.20%, the mass fraction of Mn is 0.60% to 1.40%, the mass fraction of Cr does not exceed 0.25%, the mass fraction of V does not exceed 0.20%, the mass fractions of P and S do not exceed 0.040%, the mass fraction of Al does not exceed 0.004%, and the remainder is iron and unavoidable impurities.
[0027] Flash welding primarily refers to a method of heating the rail section to be welded using resistance heating until a predetermined temperature is reached, followed by rapid application of upsetting force to achieve atomic bonding between the rail sections. The flash welding process includes four stages: electrode clamping, electrical heating, pressure upsetting, and rapid joint removal. During the welding process, the temperature of the rail sections 0mm to 25mm from the end face is 900℃ to 1800℃, and the welding duration is 50s to 300s. Specifically, in the electrode clamping stage, electrode clamping ensures the stability of the rail end during welding, preventing welding defects caused by vibration or displacement. In the electrical heating stage, the rail end is heated to 900℃ to 1800℃ for 50s to 300s, allowing it to achieve sufficient plasticity and providing favorable conditions for subsequent upsetting. In the pressure upsetting stage, upsetting force is applied at high temperature, causing plastic deformation of the rail end and achieving atomic bonding, forming a strong welded joint. Rapid weld bead removal stage: After welding is completed, excess weld beads are removed by rapid weld bead removal to ensure a smooth surface of the weld joint, reduce stress concentration points, and improve the fatigue performance of the weld joint.
[0028] Compared with existing technologies, this application significantly improves the hardness and toughness of the softened zone of the flash welded rail joint by subjecting it to secondary heating and accelerated cooling after post-weld cooling to a certain temperature, thereby reducing the low-slump phenomenon of the welded joint. The optimized heat treatment process can effectively improve the microstructure of the welded joint, reduce the occurrence of unfavorable structures such as martensite, thereby improving the overall performance of the welded joint and extending its service life. Furthermore, the width of the softened zone on one side of the flash welded rail joint treated by the above method can be controlled to less than 5mm, a significant reduction compared to traditional processes. The average hardness of the softened zone is more than 95% higher than that of the post-weld air-cooled joint, approaching the hardness level of the base material.
[0029] In some embodiments, the initial temperature of the entire heating process is <300°C, and the final temperature of the entire heating process is 900°C to 1100°C; the preset temperature is the final temperature of the entire heating process. The low initial temperature (<300°C) of this application ensures that the welded joint is in a relatively low temperature state before heating, avoiding thermal stress concentration caused by excessive temperature difference. The final temperature is set at 900°C to 1100°C to allow the metal in the welded joint area to reach the austenitizing temperature, thereby improving its microstructure through subsequent cooling processes. By precisely controlling the heating final temperature, the grain size can be effectively refined, improving the hardness and toughness of the welded joint, making its properties close to those of the base material. Simultaneously, it avoids coarse grains or overheated structures caused by excessively high temperatures, thereby improving the overall mechanical properties of the welded joint.
[0030] In some embodiments, the initial temperature of the normal heating stage is <300°C, the final temperature of the normal heating stage is 500°C to 600°C, and the duration is ≤100 seconds. This aims to rapidly increase the overall temperature of the weld joint, providing a base temperature for subsequent special heating stages. This rapid heating method can reduce the width of the heat-affected zone while avoiding the adverse effects of prolonged high temperatures on the base material properties. Rapid heating effectively reduces the width of the softened zone in the weld joint, while simultaneously improving the hardness and strength of the weld joint.
[0031] In some embodiments, during a special heating phase, the temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating phase is ≤20°C, until the final temperature of the entire heating process is reached, thus avoiding overheating or underheating in localized areas and ensuring the uniformity and stability of the heating process. Precise heating by the auxiliary heating device can further refine the microstructure of the welded joint at the rail head, improving its hardness and toughness. Simultaneously, a uniform heating process can reduce residual stress in the welded joint, improving its fatigue resistance and service performance in the softened zone of the joint.
[0032] In some embodiments, a single heating device employs an induction coil with a profile mimicking that of a steel rail, utilizing the principle of electromagnetic induction to heat the entire cross-section of the flash welded joint. The induction coil, mimicking the rail profile, is positioned 5mm to 50mm from the rail surface, and the heating area covers the entire weld joint region, including the fusion line, heat-affected zone, and base material region. This design enables rapid and efficient heating while ensuring uniform temperature distribution. The length 'a' of the heating device along the rail's extension direction is 60mm to 150mm. During the normal heating phase, the single heating device controls the temperature rise rate of the entire cross-section of the flash welded joint to be 1.0℃ / s to 20.0℃ / s, effectively refining the grains in the weld joint region, reducing residual stress, and ensuring a more uniform temperature distribution across the entire cross-section.
[0033] In some embodiments, during the special heating stage, the auxiliary heating device heats the areas at both ends of the welded joint area, specifically the rail head working area, including the rail top surface, rail head fillet, and rail head side. Since the rail head area is the contact area with the wheels after the rail is placed on the railway, its hardness requirement is higher than that of non-wheel contact areas such as the rail web and rail base. The rail web and rail base areas, primarily for support, require higher toughness; ordinary heating can achieve the desired improvement in toughness, therefore only the rail head area needs auxiliary heating.
[0034] In some embodiments, the length e of the auxiliary heating device along the rail extension direction is 20mm to 30mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the single heating device. This effectively compensates for potential temperature unevenness during the ordinary heating stage, concentrates heating on the critical working area of the rail head, and ensures temperature consistency throughout the welded joint area. The duration of auxiliary heating is <40s to effectively reduce the width of the heat-affected zone (HAZ). Short-duration high-temperature heating can prevent excessive heat diffusion, thereby reducing performance degradation caused by coarse grains in the HAZ.
[0035] In some embodiments, the average cooling rate of accelerated cooling is 5°C / s to 35°C / s, and the termination temperature of accelerated cooling is 200°C to 400°C. Accelerated cooling can rapidly reduce the temperature of the weld joint, promoting grain refinement. A fine grain structure can significantly improve the hardness, toughness, and fatigue resistance of the weld joint.
[0036] In some embodiments, the local area of the flash welded joint of the rail cooled by the cooling device includes a transition region between the heated area and the unheated base material area during the heating process, wherein the width of the base material area on each side as described in this application is 5.0 mm to 20.0 mm. When heated to the termination temperature of the entire heating process, the temperature of the local area of the flash welded joint of the rail is 400°C to 600°C.
[0037] In some embodiments, the cooling device is a contact-type heat-conducting device that mimics the profile of a rail. It utilizes heat conduction to cool both sides of the fusion line of the flash welded joint, including the entire rail head area, such as the rail top surface, rail head fillet, and rail head side, thereby achieving rapid cooling and reducing the time the welded joint remains at high temperatures. The cooling device has a hollow structure, with heat exchange occurring internally through a cooling medium. The contact surface between the cooling device and the rail is coupled using a flexible thermally conductive material. Specifically, the cooling device is equipped with cooling medium inlets and outlets to allow the cooling medium to circulate within the device. This circulation system continuously removes heat from the welded joint, ensuring the stability and efficiency of the cooling process.
[0038] In some embodiments, the cooling device includes a first cooling section that contacts the top surface of the rail head, and a second cooling section that contacts the rail head fillet and the side surface of the rail head. The thickness d of the first and second cooling sections is 15mm to 30mm, and the length b along the rail extension direction is 20mm to 40mm. The width c = the width of the rail head + 2d. The dimensional parameters of the cooling device (such as thickness d, length b, and width c) can be adjusted according to the specific shape of the rail to ensure that the cooling device fits tightly against the rail surface. This design improves the versatility and adaptability of the cooling device, making it suitable for various rail types. Figure 1 As shown, when cooling the same flash welded joint of a rail, two cooling devices are used simultaneously. By having two cooling devices work together, the cooling efficiency can be significantly improved, while ensuring the uniformity of the cooling process.
[0039] The method for improving the service performance of the softened zone of flash welded joints of rails provided in this application will be further explained below with reference to specific embodiments: Example 1 In this embodiment, the pearlitic steel rail has a C element mass fraction of 0.80%, a Si element mass fraction of 1.20%, a Mn element mass fraction of 1.10%, a Cr element mass fraction of 0.12%, a V element mass fraction of 0.05%, a P element mass fraction of 0.005%, a S element mass fraction of 0.005%, and an Al element mass fraction of 0.001%. The flash welding process mainly consists of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasts for 130 seconds. After the welding process ends and the joint cools to below 300°C, a single induction coil with a profile similar to that of the steel rail is used to perform ordinary stage heating on the entire cross-section of the flash welded joint. The induction coil with the profile similar to that of the steel rail is 5 mm away from the surface of the steel rail, the heating area covers the entire welded joint area, its length 'a' along the extension direction of the steel rail is 60 mm, the duration is 80 seconds, and the temperature rise rate is 1.0°C / s. When the rail joint temperature reaches 500℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 15℃. The length e of the auxiliary heating device along the rail extension direction is 20mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 30s. When the heating temperature reaches 900℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of a local area of the flash welded rail joint. The length b of the cooling device along the rail extension direction is 20mm, the thickness d is 15mm, and the average cooling rate for accelerated cooling is 5℃ / s. When the rail joint temperature drops to 200℃, the welded joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method is 99% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint is 2mm, which greatly improves the overall service performance of the softened zone of the flash welded rail joint.
[0040] Example 2 In this embodiment, the pearlitic steel rail has a C element mass fraction of 0.80%, a Si element mass fraction of 1.20%, a Mn element mass fraction of 1.10%, a Cr element mass fraction of 0.12%, a V element mass fraction of 0.05%, a P element mass fraction of 0.005%, a S element mass fraction of 0.005%, and an Al element mass fraction of 0.001%. The flash welding process mainly consists of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasts for 130 seconds. After the welding process ends and the joint cools to below 300°C, a single induction coil with a profile similar to that of the steel rail is used to perform ordinary stage heating on the entire cross-section of the flash welded joint. The induction coil with the profile similar to that of the steel rail is 50 mm away from the surface of the steel rail, the heating area covers the entire welded joint area, its length 'a' along the extension direction of the steel rail is 150 mm, the duration is 90 seconds, and the temperature rise rate is 20.0°C / s. When the rail joint temperature reaches 600℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 15℃. The length e of the auxiliary heating device along the rail extension direction is 30mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 30s. When the heating temperature reaches 1100℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of the flash welded rail joint in a local area. The length b of the cooling device along the rail extension direction is 40mm, the thickness d is 30mm, and the average cooling rate for accelerated cooling is 35℃ / s. When the rail joint temperature drops to 400℃, the joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method is 98% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint is 3mm, which greatly improves the overall service performance of the softened zone of the flash welded rail joint.
[0041] Example 3 In this embodiment, the pearlitic steel rail has a C element mass fraction of 0.80%, a Si element mass fraction of 1.20%, a Mn element mass fraction of 1.10%, a Cr element mass fraction of 0.12%, a V element mass fraction of 0.05%, a P element mass fraction of 0.005%, a S element mass fraction of 0.005%, and an Al element mass fraction of 0.001%. The flash welding process mainly consists of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasts for 130 seconds. After the welding process ends and the joint cools to below 300°C, a single induction coil with a profile similar to that of the steel rail is used to perform ordinary stage heating on the entire cross-section of the flash welded joint. The induction coil with the profile similar to that of the steel rail is 15 mm away from the surface of the steel rail, the heating area covers the entire welded joint area, its length 'a' along the extension direction of the steel rail is 100 mm, the duration is 80 seconds, and the temperature rise rate is 15.0°C / s. When the rail joint temperature reaches 550℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 10℃. The length e of the auxiliary heating device along the rail extension direction is 15mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 30s. When the heating temperature reaches 1000℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of the flash welded rail joint in a local area. The length b of the cooling device along the rail extension direction is 30mm, the thickness d is 20mm, and the average cooling rate for accelerated cooling is 30℃ / s. When the rail joint temperature drops to 300℃, the joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method is 98% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint is 3mm, which greatly improves the overall service performance of the softened zone of the flash welded rail joint.
[0042] Example 4 In this embodiment, the pearlitic steel rail has a C element mass fraction of 0.80%, a Si element mass fraction of 1.20%, a Mn element mass fraction of 1.10%, a Cr element mass fraction of 0.12%, a V element mass fraction of 0.05%, a P element mass fraction of 0.005%, a S element mass fraction of 0.005%, and an Al element mass fraction of 0.001%. The flash welding process mainly consists of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasts for 130 seconds. After the welding process ends and the joint cools to below 300°C, a single induction coil with a profile similar to that of the steel rail is used to perform ordinary stage heating on the entire cross-section of the flash welded joint. The induction coil with the profile similar to that of the steel rail is 5 mm away from the surface of the steel rail, the heating area covers the entire welded joint area, its length 'a' along the extension direction of the steel rail is 60 mm, the duration is 80 seconds, and the temperature rise rate is 1.0°C / s. When the rail joint temperature reaches 500℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 10℃. The length e of the auxiliary heating device along the rail extension direction is 30mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 20s. When the heating temperature reaches 1100℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of the flash welded rail joint in a local area. The length b of the cooling device along the rail extension direction is 40mm, the thickness d is 30mm, and the average cooling rate for accelerated cooling is 35℃ / s. When the rail joint temperature drops to 400℃, the joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method is 99% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint is 4mm, which greatly improves the overall service performance of the softened zone of the flash welded rail joint.
[0043] Example 5 In this embodiment, the pearlitic steel rail has a C element mass fraction of 0.80%, a Si element mass fraction of 1.20%, a Mn element mass fraction of 1.10%, a Cr element mass fraction of 0.12%, a V element mass fraction of 0.05%, a P element mass fraction of 0.005%, a S element mass fraction of 0.005%, and an Al element mass fraction of 0.001%. The flash welding process mainly consists of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasts for 130 seconds. After the welding process ends and the joint cools to below 300°C, a single induction coil with a profile similar to that of the steel rail is used to perform ordinary stage heating on the entire cross-section of the flash welded joint. The induction coil with the profile similar to that of the steel rail is 50 mm away from the surface of the steel rail, the heating area covers the entire welded joint area, its length 'a' along the extension direction of the steel rail is 150 mm, the duration is 80 seconds, and the temperature rise rate is 20.0°C / s. When the rail joint temperature reaches 600℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 15℃. The length e of the auxiliary heating device along the rail extension direction is 30mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 30s. When the heating temperature reaches 1100℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of the flash welded rail joint in a local area. The length b of the cooling device along the rail extension direction is 20mm, the thickness d is 15mm, and the average cooling rate for accelerated cooling is 5℃ / s. When the rail joint temperature drops to 200℃, the joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method is 99% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint is 4mm, which greatly improves the overall service performance of the softened zone of the flash welded rail joint.
[0044] Comparative Example 1 In this comparative example, the pearlitic steel rail used had a C content of 0.80%, a Si content of 1.20%, a Mn content of 1.10%, a Cr content of 0.12%, a V content of 0.05%, a P and S content of 0.005%, and an Al content of 0.001%. The flash welding process mainly consisted of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasted 130 seconds. After the welding process ended and the joint cooled to below 300°C, a single induction coil with a profile similar to the rail was used to heat the entire cross-section of the flash welded joint in a normal stage. The induction coil, with its profile similar to the rail, was 3 mm from the rail surface, covering the entire welded joint area. Its length 'a' along the rail's extension direction was 50 mm, the heating duration was 120 seconds, and the temperature rise rate was 0.5°C / s. When the rail joint temperature reaches 400℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 25℃. The length e of the auxiliary heating device along the rail extension direction is 10mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 50s. When the heating temperature reaches 800℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of the flash welded rail joint in a local area. The length b of the cooling device along the rail extension direction is 10mm, the thickness d is 10mm, and the average cooling rate for accelerated cooling is 4℃ / s. When the rail joint temperature drops to 100℃, the joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method was only 30% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint was 22mm. The joint performance could not meet the requirements.
[0045] Comparative Example 2 In this comparative example, the pearlitic steel rail used had a C content of 0.80%, a Si content of 1.20%, a Mn content of 1.10%, a Cr content of 0.12%, a V content of 0.05%, a P and S content of 0.005%, and an Al content of 0.001%. The flash welding process mainly consisted of four stages: electrode clamping, electric heating, pressure upsetting, and rapid sulphur pushing. The entire welding process lasted 130 seconds. After the welding process ended and the joint cooled to below 300°C, a single induction coil with a profile similar to the rail was used to heat the entire cross-section of the flash welded joint in a normal stage. The induction coil, with its profile similar to the rail, was 55 mm from the rail surface, covering the entire welded joint area. Its length 'a' along the rail's extension direction was 155 mm, the heating duration was 110 seconds, and the temperature rise rate was 25.0°C / s. When the rail joint temperature reaches 650℃, an auxiliary heating device is used to heat the area on both sides of the fusion line of the flash welded rail joint (including the rail top surface, rail head fillet, and rail head side). The temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating stage is 25℃. The length e of the auxiliary heating device along the rail extension direction is 35mm, and the centerline of the area covered by the auxiliary heating device coincides with the edge of the area covered by the single heating device. The duration of auxiliary heating is 50s. When the heating temperature reaches 1200℃, the single heating device and the auxiliary heating device are immediately removed, and a contact heat conduction device with a rail profile is used to cool the rail head of the flash welded rail joint in a local area. The length b of the cooling device along the rail extension direction is 45mm, the thickness d is 35mm, and the average cooling rate for accelerated cooling is 40℃ / s. When the rail joint temperature drops to 500℃, the joint is placed in the air to cool naturally. The average hardness of the softened zone of the flash welded rail joint treated with this method was only 50% higher than that of the air-cooled joint after welding, and the width of the softened zone on one side of the joint was 30mm. The joint performance could not meet the requirements.
[0046] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0047] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A method for improving the service performance of the softened zone of a flash-welded rail joint, characterized in that: include: The flash welded joints of the rails, after cooling to a certain temperature following welding, undergo secondary heating. The heating process includes a normal heating stage and a special heating stage. In the normal heating stage, a single heating device is used to heat the entire cross-section of the flash welded joint. In the special heating stage, a single heating device is used to continue heating the entire cross-section of the flash welded joint, while an auxiliary heating device is used to supplement the heating of the rail heads at both ends of the area covered by the single heating device. The area supplemented by the auxiliary heating device is the working area of the rail head, including the top surface of the rail, the rounded corners of the rail head, and the side surface of the rail head, and the centerline of the area covered by the auxiliary heating device coincides with the edge covered by the single heating device. After the rail flash welded joint is heated to the preset temperature, the single heating device and the auxiliary heating device are immediately removed, and a cooling device is used to accelerate the cooling of the local area on both sides of the fusion line of the rail flash welded joint that has been heated to the preset temperature.
2. The method according to claim 1, characterized in that: The starting temperature of the entire heating process is <300℃, and the ending temperature of the entire heating process is 900℃~1100℃; the preset temperature is the ending temperature of the entire heating process.
3. The method according to claim 2, characterized in that: The starting temperature of the normal heating stage is <300℃, the ending temperature of the normal heating stage is 500℃~600℃, and the duration is ≤100s.
4. The method according to claim 3, characterized in that: During the special heating phase, the temperature difference between the starting temperature of the auxiliary heating device and the ending temperature of the normal heating phase is ≤20℃, until the end temperature of the entire heating process is reached and the process ends.
5. The method according to claim 1, characterized in that: The single heating device employs an induction coil with a profile similar to that of a steel rail. The distance between the induction coil and the surface of the steel rail is 5mm to 50mm, and the heating area covers the entire welded joint area. The length of the single heating device along the extension direction of the steel rail is 60mm to 150mm. During the normal heating stage, the single heating device controls the temperature rise rate of the entire cross-section of the flash welded joint of the steel rail to be 1.0℃ / s to 20.0℃ / s.
6. The method according to claim 5, characterized in that: During the special heating stage, the auxiliary heating device assists in heating the areas at both ends of the weld joint area.
7. The method according to claim 6, characterized in that: The length of the auxiliary heating device along the extension direction of the rail is 20mm to 30mm, and the duration of auxiliary heating is <40s.
8. The method according to claim 1, characterized in that: The average cooling rate of the accelerated cooling is 5℃ / s to 35℃ / s, and the termination temperature of the accelerated cooling is 200℃ to 400℃.
9. The method according to claim 1, characterized in that: The local area cooled by the cooling device includes the transition area between the heated area and the unheated joint base material area during the heating process. When heated to the termination temperature of the entire heating process, the temperature of the local area is 400℃~600℃.
10. The method according to claim 1, characterized in that: The cooling device is a contact-type heat-conducting device that mimics the profile of a steel rail. The cooling device has a hollow structure and heat exchange occurs internally through a cooling medium. The cooling device is coupled to the steel rail contact surface using a flexible heat-conducting material.
11. The method according to claim 10, characterized in that: The cooling device includes a first cooling section that contacts the top surface of the rail head and a second cooling section that contacts the rounded corners and side surfaces of the rail head. The thickness of the first and second cooling sections is 15mm to 30mm, and their length along the extension direction of the rail is 20mm to 40mm.
Citation Information
Patent Citations
Fixed flash welding and joint heat treatment method for 75kg / m hypereutectoid steel rail for heavy haul railway
CN116237624A