High-thermal-conductivity wear-resistant hot-corrosion-resistant high-entropy alloy coating with multi-layer structure and preparation method thereof
By preparing a multi-layer structure with a high thermal conductivity, wear resistance, heat corrosion resistance, high entropy alloy coating with a multi-layer structure on the surface of the boiler pipe, the problem of thermal corrosion and wear easily occurring in the high temperature environment of the boiler pipe is solved, and efficient thermal conductivity, wear resistance and heat corrosion resistance are achieved, reducing the preparation cost and process complexity.
Patent Information
- Application Number
- CN202510536473.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-27
- Publication Date
- 2025-05-27
- Estimated Expiration
- 2045-04-27
AI Technical Summary
The surface of the boiler pipe is prone to thermal corrosion and high-temperature wear in a high-temperature environment, resulting in a decrease in thermal conductivity, a decrease in mechanical strength and equipment safety hazards. The existing high-entropy alloy powder preparation process is costly and complicated.
A high thermal conductivity, wear-resistant and heat corrosion-resistant high-entropy alloy coating with a multi-layer structure, including NiCr adhesive layer, AlCoCrNiMo high-entropy alloy transition layer, AlCoCrNiMoBSi high-entropy alloy functional layer and nitriding modified layer, was prepared by oxygen-kerosene supersonic flame spraying and solid solution-aging treatment, and combined with nitriding treatment to form a dense nitriding layer.
It significantly improves the thermal conductivity, wear resistance and heat corrosion resistance of the boiler tube surface, reduces the cost and process complexity of coating preparation, extends the service life of the equipment and improves safety.
Smart Images

Figure CN120041774A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical fields of thermal spraying and surface nitriding, and particularly relates to a multi-layered high thermal conductivity, anti-wear, heat corrosion-resistant high-entropy alloy coating and a preparation method thereof. Background Art
[0002] As a core device in the thermal power generation system, the boiler tube wall in a boiler is a key component for efficient heat transfer. Its main function is to quickly conduct heat to the water-cooling system to drive power generation by directly contacting with high-temperature flue gas and molten substances. Under the harsh working conditions of long-term exposure to temperatures above 600 °C, sulfide corrosion media, and ash particle erosion on the surface of the boiler tube, thermal corrosion and high-temperature wear are extremely likely to occur. This will not only reduce the heat conduction efficiency of the tube wall, but also lead to a decrease in the mechanical strength of the tube wall, trigger tube burst accidents, and shorten the equipment maintenance cycle. Therefore, it is urgent to strengthen the surface of the boiler tube by preparing a protective coating with high thermal conductivity, anti-wear, and heat corrosion-resistant characteristics to improve its service performance and service life in a complex thermal environment.
[0003] The advantage of AlCoCrNiMo high-entropy alloy as a heat corrosion-resistant protective coating lies in its multi-principal element synergistic effect and microstructure design. Al and Cr cooperate to form an Al 2 O 3 / Cr 2 O 3 double-layer passivation film. Combining with the unique diffusion retardation effect of high-entropy alloy, it significantly inhibits the penetration of oxygen and corrosion media, and the introduction of Mo further strengthens the denseness of the passivation film. In addition, the ordered phase in the AlCoCrNi-based high-entropy alloy can reduce lattice distortion and phonon scattering, thereby improving the thermal conductivity. Research shows that its room-temperature thermal conductivity is significantly better than that of traditional stainless steel. It is reported that B and Si elements in the alloy will preferentially oxidize to form B 2 O 3 and SiO 2 or form composite oxides with other elements (such as Al, Cr). Such oxide films have denseness and high stability, and can also block the penetration of corrosive media. Therefore, introducing B and Si elements into AlCoCrNiMo high-entropy alloy can further improve its anti-thermal corrosion performance. To cope with potential wear failure during service, a dense nitride layer is formed on the surface of the high-entropy alloy by nitriding treatment. Based on the multi-principal element characteristics of the high-entropy alloy, it promotes the formation of multi-component nitride phases, and realizes solid solution strengthening and dispersion strengthening at the nanoscale, improves the bearing capacity of the nitride layer, and inhibits crack initiation and propagation, thereby improving the friction and wear performance of the material.
[0004] Since the AlCoCrNiMoBSi high-entropy alloy contains high melting point elements (such as Mo, 2623 °C, B, 2180 °C) and low melting point elements (such as Al, 660 °C, Si, 1414 °C). During melting, high temperatures may cause low melting point elements such as Al and Si to volatilize, resulting in a deviation of the composition from the designed ratio. In addition, the preparation of traditional high-entropy alloy powders involves melting and spray granulation, which has the disadvantages of strict process parameter requirements and high energy consumption, limiting the application of thermal sprayed high-entropy alloy coatings in the field of boiler tube protection. Summary of the Invention
[0005] The purpose of the present invention is to solve the problems of poor thermal conductivity, insufficient heat-resistant corrosion and friction and wear resistance of the protective coating for ordinary boiler tubes, and the high cost and complex process of preparing traditional high-entropy alloy powders, and to provide a multi-layered high-thermal-conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating and its preparation method.
[0006] To achieve the above purpose, the present invention discloses a multi-layered high-thermal-conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating, and the multi-layered high-thermal-conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating includes a NiCr bonding layer in the first layer, an AlCoCrNiMo high-entropy alloy transition layer in the second layer, an AlCoCrNiMoBSi high-entropy alloy functional layer in the third layer, and a nitriding modification layer in the fourth layer.
[0007] The thickness of the NiCr bonding layer is 40 - 60 μm, the thickness of the AlCoCrNiMo high-entropy alloy transition layer is 60 - 80 μm, the thickness of the AlCoCrNiMoBSi high-entropy alloy functional layer is 160 - 200 μm, and the thickness of the nitriding modification layer is 2 - 3 μm.
[0008] The present invention also discloses a preparation method of the above multi-layered high-thermal-conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating, including the following steps:
[0009] S1, spraying NiCr powder on the surface of the sandblasted substrate by oxy-kerosene supersonic flame to prepare the NiCr bonding layer;
[0010] S2, spraying the solution-treated and aged AlCoCrNiMo high-entropy alloy powder on the surface of the NiCr bonding layer by oxy-kerosene supersonic flame to prepare the AlCoCrNiMo high-entropy alloy transition layer;
[0011] S3, spraying the solution-treated and aged AlCoCrNiMoBSi high-entropy alloy powder on the surface of the AlCoCrNiMo high-entropy alloy transition layer by oxy-kerosene supersonic flame to prepare the AlCoCrNiMoBSi high-entropy alloy functional layer;
[0012] S4. Perform nitriding treatment on the surface of the polished and ground AlCoCrNiMoBSi high-entropy alloy functional layer to obtain a high-thermal-conductivity, anti-wear, and heat-resistant corrosion high-entropy alloy coating with a multi-layer structure.
[0013] In the steps S2 and S3, the solution-aging treatment specifically includes the following steps:
[0014] A1. Place the AlCoCrNiMo alloy powder or AlCoCrNiMoBSi alloy powder in a vacuum heat treatment furnace, close the furnace lid, and evacuate the inside of the vacuum heat treatment furnace to below 10 -5 Pa.
[0015] A2. After evacuating to 10 -5 Pa, heat it up to 1150°C at a heating rate of 10°C / min and hold for 5 h to perform solution treatment on the AlCoCrNiMo alloy powder or AlCoCrNiMoBSi alloy powder. The solution treatment temperature is 1150°C and the solution treatment time is 5 h.
[0016] A3. After the solution treatment is completed, cool it down to 600°C and hold for 4 h to perform aging treatment on the AlCoCrNiMo alloy powder or AlCoCrNiMoBSi alloy powder. The aging treatment temperature is 600°C and the aging treatment time is 4 h.
[0017] A4. After the aging treatment is completed, maintain the vacuum degree inside the furnace cavity and cool it down to room temperature with the furnace to finally obtain AlCoCrNiMo high-entropy alloy powder or AlCoCrNiMoBSi high-entropy alloy powder.
[0018] In the step A1, the preparation method of the AlCoCrNiMo alloy powder is as follows: First, ball-mill the elemental Cr and Mo powders for 25 h, then add the elemental Co powder and ball-mill for 35 h, and then add the elemental Al and Ni powders and ball-mill for 45 h. The molar ratio of the elemental powder elements of the AlCoCrNiMo alloy powder is Al:Co:Cr:Ni:Mo = 1:1:1:1:1, and the particle sizes of the elemental Al, Co, Cr, Ni, and Mo powders are 15 - 45 μm.
[0019] In the step A1, the preparation method of the AlCoCrNiMoBSi alloy powder is as follows: First, the elemental Cr and Mo powders are ball-milled for 25 h, then the elemental Co powder is added and ball-milled for 35 h, the elemental Al and Ni powders are added and ball-milled for 45 h, and then the elemental B and Si powders are added and ball-milled for 55 h; the molar ratio of the elemental powders of the AlCoCrNiMoBSi alloy powder is Al:Co:Cr:Ni:Mo:B:Si = 1:1:1:1:1:0.1:0.15. The particle sizes of the elemental Al, Co, Cr, Ni, and Mo powders are 15 - 45 μm, and the particle sizes of the elemental B and Si powders are 1 - 3 μm.
[0020] In the step S2, the process parameters of the oxygen-kerosene supersonic flame spraying are as follows: the kerosene flow rate is 26 m 3 / h, the oxygen flow rate is 53 m 3 / h, the spraying distance is 380 mm, the spraying step distance is 3 mm, the moving speed of the spray gun is 800 mm / s, the barrel size is 6 inches, the powder feeding rate is 50 g / min, and it is sprayed for 2 - 3 passes.
[0021] In the step S3, the process parameters of the oxygen-kerosene supersonic flame spraying are as follows: the kerosene flow rate is 32 m 3 / h, the oxygen flow rate is 53 m 3 / h, the spraying distance is 380 mm, the spraying step distance is 3 mm, the moving speed of the spray gun is 800 mm / s, the barrel size is 6 inches, the powder feeding rate is 50 g / min, and it is sprayed for 3 - 5 passes.
[0022] In the step S4, the process parameters of the oxygen-kerosene supersonic flame spraying are as follows: the kerosene flow rate is 32 m 3 / h, the oxygen flow rate is 53 m 3 / h, the spraying distance is 380 mm, the spraying step distance is 3 mm, the moving speed of the spray gun is 800 mm / s, the barrel size is 6 inches, the powder feeding rate is 50 g / min, and it is sprayed for 8 - 15 passes.
[0023] In the step S4, the specific steps of the nitriding treatment are as follows:
[0024] B1, Put the sample to be nitrided into the nitriding furnace and seal the furnace body; evacuate the nitriding furnace to below 5 Pa before formal nitriding;
[0025] B2, Heating stage: After the nitriding furnace reaches the predetermined vacuum degree, adjust the nitrogen / hydrogen gas flow rate to make the gas pressure in the furnace 60 - 80 Pa, increase the power supply voltage to 450 V, and simultaneously introduce nitrogen / hydrogen gas flow. According to the arc state inside the nitriding furnace, slowly adjust the voltage and conduction ratio to make the temperature inside the furnace rise and maintain a stable glow. When the temperature reaches 300 °C, turn on the furnace body cooling water to cool the furnace wall until the temperature rises to the preset temperature of 600 °C;
[0026] B3, Insulation stage: After the nitriding furnace reaches the preset temperature, control the voltage at 720 V, the nitrogen gas flow rate at 600 sccm, the hydrogen gas flow rate at 200 sccm, and the duty cycle at 3:1 to ensure the stability of the temperature and pressure inside the furnace. The insulation stage lasts for 8 - 48 h;
[0027] B4, Cooling stage: After the insulation is completed, turn off the power supply and continue to introduce nitrogen / hydrogen gas, with the nitrogen gas flow rate at 600 sccm and the hydrogen gas flow rate at 200 sccm, to maintain the reducing atmosphere inside the nitriding furnace to prevent oxidation, and cool with the furnace to finally obtain a high - thermal - conductivity, anti - wear, heat - resistant and corrosion - resistant high - entropy alloy coating with a multi - layer structure.
[0028] The beneficial effects of the present invention compared with the prior art are as follows:
[0029] 1. The AlCoCrNiMo high - entropy alloy powder and AlCoCrNiMoBSi high - entropy alloy powder prepared by the present invention through step - by - step mechanical alloying and solution - aging treatment achieve forced alloying of multi - element metals in the solid state by high - energy ball milling, avoiding the limitation of the traditional melting process on the melting point difference of components. During the step - by - step mechanical alloying process, the powder undergoes repeated cold welding - crushing to achieve nano - level uniform mixing, and then through solution - aging treatment, lattice distortion is eliminated and solid solution strengthening is formed, finally obtaining high - entropy alloy powder with a dual - phase BCC / FCC structure. Compared with the traditional melting + atomization granulation method, this process has the characteristics of simple process, environmental friendliness, and low cost;
[0030] 2. The present invention utilizes the high thermal conductivity and heat - resistant and corrosion - resistant properties of the high - entropy alloy itself to prepare a high - thermal - conductivity, anti - wear, heat - resistant and corrosion - resistant high - entropy alloy coating with a multi - layer structure on the surface of the boiler tube. Among them, the NiCr bonding layer has high compatibility with the substrate, can enhance the interfacial bonding strength, block the diffusion of substrate elements, and maintain the stability of the coating; the AlCoCrNiMo high - entropy alloy transition layer and the AlCoCrNiMoBSi high - entropy alloy functional layer have similar compositions, can relieve interfacial stress, reduce the thermal expansion coefficient gradient difference, and inhibit the cracking or spalling of the functional layer;
[0031] 3. During the nitriding process of the present invention, the Al, Cr, and Mo elements in the AlCoCrNiMoBSi high - entropy alloy functional layer combine with nitrogen to form hard nitrides. These dense nitride layers and the oxide film (such as Al 2O 3 and Cr 2 O 3 etc.) have the characteristics of self-lubrication, high hardness, and oxygen diffusion hindrance, and can achieve the functions of friction reduction and corrosion resistance; at the same time, nitrogen atoms diffuse into the coating to occur atomic-level diffusion and form residual compressive stress. This metallurgical bonding and residual stress state inhibit the initiation and spalling of cracks, avoid the spalling of the nitrided layer, and thus achieve the long-term anti-wear and heat-resistant corrosion effects. Description of the Drawings
[0032] Figure 1 is the SEM image of AlCoCrNiMoBSi alloy powder;
[0033] Figure 2 is the SEM image of AlCoCrNiMoBSi high-entropy alloy powder;
[0034] Figure 3 is the XRD pattern of AlCoCrNiMoBSi alloy powder and AlCoCrNiMoBSi high-entropy alloy powder;
[0035] Figure 4 is the SEM image of the high-thermal conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating with a multi-layer structure;
[0036] Figure 5 is Figure 4 the partial enlarged view of point A in
[0037] Figure 6 is the schematic diagram of the structure of the high-thermal conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating with a multi-layer structure. Detailed Embodiments
[0038] The following further elaborates on the above and other technical features and advantages of the present invention with reference to the drawings.
[0039] Example 1
[0040] A preparation method of AlCoCrNiMoBSi high-entropy alloy powder includes first preparing AlCoCrNiMoBSi alloy powder by step-by-step mechanical alloying; then subjecting the AlCoCrNiMoBSi alloy powder to solution-aging treatment to prepare AlCoCrNiMoBSi high-entropy alloy powder.
[0041] The above-mentioned step-by-step mechanical alloying preparation process of AlCoCrNiMoBSi alloy powder includes the following steps:
[0042] (1)First, weigh the elemental Al, Co, Cr, Ni, Mo, B, and Si powders used for the preparation of AlCoCrNiMoBSi alloy powder by stepwise mechanical alloying. The molar ratio is Al:Co:Cr:Ni:Mo:B:Si = 1:1:1:1:1:0.1:0.15, and calculate the total mass of these elemental powders.
[0043] (2)Pour the weighed elemental Cr and Mo powders into the ball milling tank, add mixed grinding balls into the ball milling tank. The size and mass ratio of the mixed grinding balls are 15mm:10mm:6mm:5mm = 1:4:2:1, and the ratio of the total mass of the mixed grinding balls to the total mass of the elemental powders is 10:1; then seal the ball milling tank, and perform vacuum pumping and argon filling on the inside of the tank body. The vacuum degree should be below 10 Pa, and the argon filled is high-purity argon with a pressure of 0.2 - 0.3 MPa, and the filling time is 15 min.
[0044] (3)Place the ball milling tank in an all-round planetary ball mill, set the ball milling speed to 220 rpm, with a cycle of 10 min of forward rotation, 2 min of shutdown, 10 min of reverse rotation, and 2 min of shutdown, and the ball milling time is 25 h.
[0045] (4)After ball milling for 25 h, open the ball milling tank and pour in the weighed elemental Co powder, and perform the sealing, vacuum pumping, and argon filling treatments on the ball milling tank as in step (2), and then ball mill according to the parameters in step (3) until 35 h.
[0046] (5)After ball milling for 35 h, open the ball milling tank and pour in the weighed elemental Al and Ni powders, and perform the sealing, vacuum pumping, and argon filling treatments on the ball milling tank as in step (2), and then ball mill according to the parameters in step (3) until 45 h.
[0047] (6)After ball milling for 45 h, open the ball milling tank and pour in the weighed elemental B and Si powders, and perform the sealing, vacuum pumping, and argon filling treatments on the ball milling tank as in step (2), and then ball mill according to the parameters in step (3) until 55 h.
[0048] (7)After reaching the ball milling time, take out the AlCoCrNiMoBSi alloy powder, and use a powder sieve and a metal sieve equipped with an ultrasonic vibrator to screen the powder. The upper metal sieve is 325 mesh, the lower metal sieve is 800 mesh, the ultrasonic vibrator is installed on the lower metal sieve, and the screening time is 30 min; finally, take out the AlCoCrNiMoBSi alloy powder with a particle size range of 15 - 45 μm from the lower sieve.
[0049] The solution - aging treatment of the above - mentioned AlCoCrNiMoBSi alloy powder includes the following steps:
[0050] (1) Place the AlCoCrNiMoBSi alloy powder prepared in the above steps in a corundum crucible and place it in a vacuum heat treatment furnace; close the furnace lid, turn on the mechanical pump and molecular pump to evacuate the inside of the furnace cavity to a vacuum of less than 10 -5 Pa.
[0051] (2) Solution treatment: After reaching the specified vacuum degree, heat it up to 1150 °C at a heating rate of 10 °C / min and hold for 5 h to perform solution treatment on the AlCoCrNiMoBSi alloy powder.
[0052] (3) Aging treatment: After reaching the solution treatment time, cool it down to 600 °C and hold for 4 h to perform aging treatment on the AlCoCrNiMoBSi alloy powder.
[0053] (4) After aging treatment, maintain the vacuum degree inside the furnace cavity (less than 10 -5 Pa), and cool it down to room temperature with the furnace to finally obtain AlCoCrNiMoBSi high-entropy alloy powder.
[0054] For the AlCoCrNiMoBSi alloy powder and AlCoCrNiMoBSi high-entropy alloy powder prepared in this example, use SEM to observe the cross-sectional microstructure of the powder, as Figure 1 shown; use XRD to detect the phase composition of the powder, as Figure 2 shown.
[0055] It can be seen from Figure 1 that the step-by-step mechanical alloying method can prepare elemental Al, Co, Cr, Ni, Mo, B and Si powders into uniformly distributed AlCoCrNiMoBSi alloy powders, and the AlCoCrNiMoBSi alloy powders have a spherical-like morphology and particle sizes suitable for thermal spraying. It can be seen from Figure 2 that the AlCoCrNiMoBSi high-entropy powder obtained after solution-aging treatment has similar dimensions and shapes to the AlCoCrNiMoBSi alloy powder, but the elemental distribution inside the powder is more uniform. Figure 3 The phase analysis results of
[0056] Example 2
[0057] A high thermal conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating with a multi-layer structure, as Figure 6As shown, from the bottom layer to the surface, it successively includes an oxygen-kerosene supersonic flame sprayed NiCr bonding layer, an AlCoCrNiMo high-entropy alloy transition layer, an AlCoCrNiMoBSi high-entropy alloy functional layer, and a nitriding modified layer.
[0058] The preparation processes of the above-mentioned oxygen-kerosene supersonic flame sprayed NiCr bonding layer, AlCoCrNiMo high-entropy alloy transition layer, and AlCoCrNiMoBSi high-entropy alloy functional layer include the following steps:
[0059] (1) Dry the NiCr powder, AlCoCrNiMo high-entropy alloy powder, and AlCoCrNiMoBSi high-entropy alloy powder to remove excess moisture. The drying temperature is 120 °C and the time is 20 min.
[0060] (2) Roughly sandblast the surface of the boiler steel. Use 24-mesh brown fused alumina sand, and the sandblasting carrier gas pressure is 0.5 - 0.7 MPa. After sandblasting, clean the substrate with anhydrous ethanol or acetone, and then preheat the substrate. The preheating temperature is 120 °C and the time is 15 min.
[0061] (3) Preparation of the NiCr bonding layer: The process parameters of oxygen-kerosene supersonic flame spraying include a kerosene flow rate of 26 m 3 / h, an oxygen flow rate of 53 m 3 / h, a spraying distance of 380 mm, a spraying step distance of 3 mm, a spray gun moving speed of 800 mm / s, a barrel size of 6 inches, a powder feeding rate of 50 g / min, spray 2 passes, and the thickness of the NiCr bonding layer is 40 - 60 μm.
[0062] (4) Preparation of the AlCoCrNiMo high-entropy alloy transition layer: Directly perform oxygen-kerosene supersonic flame spraying on the surface of the NiCr bonding layer. The process parameters include a kerosene flow rate of 32 m 3 / h, an oxygen flow rate of 53 m 3 / h, a spraying distance of 380 mm, a spraying step distance of 3 mm, a spray gun moving speed of 800 mm / s, a barrel size of 6 inches, a powder feeding rate of 50 g / min, spray 4 passes, and the thickness of the AlCoCrNiMo high-entropy alloy transition layer is 60 - 80 μm.
[0063] (5) Preparation of the AlCoCrNiMoBSi high-entropy alloy functional layer: Directly perform oxygen-kerosene supersonic flame spraying on the surface of the AlCoCrNiMo transition layer. The process parameters include a kerosene flow rate of 32 m 3 / h, an oxygen flow rate of 53 m 3 / h, spraying distance is 380 mm, spraying step distance is 3 mm, spray gun moving speed is 800 mm / s, barrel size is 6 inches, powder feeding rate is 50 g / min, spraying is carried out for 12 passes, and the thickness of the AlCoCrNiMoBSi functional layer is 160 - 200 μm.
[0064] The preparation process of the above nitriding modified layer includes the following steps:
[0065] (1) Before nitriding, the surface of the functional layer is polished, and the polished sample surface is thoroughly cleaned with anhydrous ethanol or acetone.
[0066] (2) The sample to be nitrided is placed in a nitriding furnace, and the furnace body is sealed; before formal nitriding, the nitriding furnace is pumped to near vacuum (below 5 Pa).
[0067] (3) Heating stage: When the nitriding furnace reaches the predetermined vacuum degree, adjust the nitrogen / hydrogen gas flow rate to make the gas pressure value in the furnace 60 - 80 Pa, increase the power supply voltage to 450 V, and at the same time introduce nitrogen / hydrogen gas flow. According to the arc light state inside the nitriding furnace, slowly adjust the voltage and conduction ratio to make the temperature in the furnace rise and maintain a stable glow. When the temperature reaches 300 °C, turn on the furnace body cooling water to cool the furnace wall until the temperature rises to the preset temperature of 600 °C.
[0068] (4) Insulation stage: When the nitriding furnace reaches the preset temperature, control the voltage to 720 V, the nitrogen gas flow rate to 600 sccm, the hydrogen gas flow rate to 200 sccm, and the duty cycle to 3:1 to ensure the stability of the temperature and pressure in the furnace. The insulation stage lasts for 8 h respectively.
[0069] (5) Cooling stage: After reaching the preset insulation time, turn off the power supply, continue to introduce nitrogen / hydrogen gas, the nitrogen gas flow rate is 600 sccm, the hydrogen gas flow rate is 200 sccm, maintain the reducing atmosphere in the nitriding furnace to prevent oxidation, and cool with the furnace to finally obtain a multi-layered high-thermal-conductivity, anti-wear, heat-resistant and corrosion-resistant high-entropy alloy coating.
[0070] For the multi-layered structure coating (before nitriding) prepared in this embodiment, a universal tensile testing machine is used to measure the bonding strength of the multi-layered structure coating, and a Vickers hardness tester is used to measure the microhardness and fracture toughness of the multi-layered structure coating. The results are shown in Table 1.
[0071] Table 1 Bonding strength and fracture toughness of the multi-layered structure coating
[0072]
[0073] As can be seen from Table 1, the bonding layer can significantly improve the bonding strength between the functional layer and the substrate, but it has little effect on the microhardness and fracture toughness of the modified layer. The composition of the transition layer is similar to that of the functional layer, which can improve the bonding strength of the functional layer to a certain extent. In addition, due to the supporting effect of the transition layer, the microhardness and fracture toughness of the double-layer structure coating of the transition layer + functional layer are significantly improved compared with the single-layer functional layer. The three-layer structure coating of the bonding layer + transition layer + functional layer combines the characteristics of the bonding layer and the transition layer, and the bonding strength, microhardness and fracture toughness of the coating are all significantly improved.
[0074] Example 3
[0075] The difference between this example and Example 2 is that in step (4) of the preparation process of the nitrided modified layer, the holding stage lasts for 16 h, and other process steps are the same as those in Example 2.
[0076] Example 4
[0077] The difference between this example and Example 2 is that in step (4) of the preparation process of the nitrided modified layer, the holding stage lasts for 32 h, and other process steps are the same as those in Example 2.
[0078] Example 5
[0079] The difference between this example and Example 2 is that in step (4) of the preparation process of the nitrided modified layer, the holding stage lasts for 48 h, and other process steps are the same as those in Example 2.
[0080] Performance tests were carried out on the multi-layer structure coatings nitrided at different times (8 h, 16 h, 32 h, 48 h) prepared in Examples 2 to 5: a laser thermal conductivity analyzer was used to measure the thermal conductivity of the coatings at different temperatures, a pin-on-disc friction and wear tester was used to measure the friction and wear performance of the coatings at 700 °C, and a precision balance was used to evaluate the weight gain of the coatings after 100 h of thermal corrosion; SEM was used to observe the cross-section of the high thermal conductivity, anti-wear and heat-resistant corrosion high-entropy alloy coating of the multi-layer structure after nitriding for 16 h, as Figure 4 and Figure 5 shown.
[0081] Figure 4 is the overall morphology diagram of the multi-layer structure coating. The coating is dense inside and has no pores. The interfaces of the multi-layer coatings are well bonded. The thickness of the NiCr bonding layer is 62 μm, the thickness of the AlCoCrNiMo high-entropy alloy transition layer is 84 μm, and the thickness of the AlCoCrNiMoBSi high-entropy alloy functional layer is 162 μm. Figure 5 is the enlarged view near the top of the multi-layer structure coating. After the nitriding surface modification treatment, a continuous and dense nitrided modified layer is formed on the coating surface, and its thickness is 2.33 μm. Figure 6Shown is a schematic diagram of the multi-layered structure coating.
[0082] The thermal conductivity of the coating at different temperatures is shown in Table 2:
[0083] Table 2 Thermal conductivity of the coating at different temperatures
[0084]
[0085] As can be seen from Table 2, the thermal conductivity of the multi-layered structure coating at room temperature is 8.86 W∙(m∙K) -1 , and as the test temperature increases, the thermal conductivity of the multi-layered structure coating gradually increases, reaching 19.89 W∙(m∙K) at 700 °C -1 , which can reach more than 80% of the thermal conductivity of the boiler steel substrate (21.13 W∙(m∙K) at 700 °C -1 ). After nitriding the multi-layered structure coating for 8 h and 16 h, the thermal conductivities at room temperature and 700 °C are comparable to those of the non-nitrided coating, indicating that the nitrided layer obtained under these nitriding parameters has little effect on the thermal conductivity of the multi-layered structure coating. When the nitriding time reaches 32 h and 48 h, the thermal conductivity of the coating decreases significantly, and the thermal conductivity at 700 °C is only less than 51% of the thermal conductivity of the boiler steel substrate, which cannot meet the requirement of high thermal conductivity.
[0086] The friction coefficient and wear rate of the coating at 700 °C are shown in Table 3 below:
[0087] Table 3 Friction coefficient and wear rate of the coating at 700 °C
[0088]
[0089] As can be seen from Table 3, after the multi-layered structure coating is nitrided for 16 h, the friction coefficient and wear rate are 0.27 and 3.72×10 -5 mm 3 ∙(N∙m) -1 , respectively, showing better anti-friction and anti-wear effects compared to the non-nitrided coating. When the nitriding time reaches 32 h and 48 h, the friction coefficient and wear rate increase slightly, but both are better than those of the non-nitrided coating.
[0090] The thermal corrosion weight gain and thermal corrosion weight gain kinetic constant for different nitriding times are shown in Table 4 below:
[0091] Table 4 Thermal corrosion weight gain and thermal corrosion weight gain kinetic constant for different nitriding times
[0092]
[0093] As can be seen from Table 4, the thermal corrosion weight gain and kinetic constant of the AlCoCrNiMoBSi high-entropy alloy multi-layer structure coating after 16 h of nitriding treatment are 4.67 mg∙cm -2 and 0.43 mg 2 ∙cm -4 ∙h -1 , respectively. The heat-resistant corrosion performance is several times higher than that of the un-nitrided coating. When the nitriding time reaches 32 h and 48 h, the heat-resistant corrosion performance of the coating is better than that of the un-nitrided coating.
[0094] Based on the comprehensive tests of the thermal conductivity, friction and wear, and heat-resistant corrosion performance of the multi-layer structure coating before and after nitriding, the following conclusions can be drawn: The multi-layer structure high-entropy alloy coating obtained after 16 h of nitriding treatment can significantly improve its friction and wear performance and heat-resistant corrosion performance while taking into account the high thermal conductivity.
[0095] The above are only the preferred embodiments of the present invention, which are illustrative rather than restrictive to the present invention. Those skilled in the art understand that many changes, modifications, and even equivalents can be made within the spirit and scope defined by the claims of the present invention, but all will fall within the protection scope of the present invention.
Claims
1. A multi-layered high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating, characterized in that: The multi-layer structure of high thermal conductivity, wear resistance, heat corrosion resistance and high entropy alloy coating comprises a first layer of NiCr bonding layer, a second layer of AlCoCrNiMo high entropy alloy transition layer, a third layer of AlCoCrNiMoBSi high entropy alloy functional layer and a fourth layer of nitriding modification layer.
2. A multi-layered high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating as claimed in claim 1, characterized in that: The thickness of the NiCr bonding layer is 40-60 μm, the thickness of the AlCoCrNiMo high entropy alloy transition layer is 60-80 μm, the thickness of the AlCoCrNiMoBSi high entropy alloy functional layer is 160-200 μm, and the thickness of the nitriding modification layer is 2-3 μm.
3. A method for preparing a multilayer high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1, spraying NiCr powder on the surface of the substrate after sandblasting by using oxygen-kerosene supersonic flame to prepare a NiCr bonding layer; S2, using oxygen-kerosene supersonic flame spraying of AlCoCrNiMo high entropy alloy powder after solid solution-aging treatment on the surface of the NiCr bonding layer to prepare an AlCoCrNiMo high entropy alloy transition layer; S3, spraying AlCoCrNiMoBSi high entropy alloy powder after solid solution-aging treatment on the surface of the AlCoCrNiMo high entropy alloy transition layer by oxygen-kerosene supersonic flame to prepare an AlCoCrNiMoBSi high entropy alloy functional layer; S4, performing nitriding treatment on the surface of the AlCoCrNiMoBSi high entropy alloy functional layer after grinding and polishing to obtain a multi-layer structure of a high thermal conductivity, wear resistance, and heat corrosion resistance high entropy alloy coating.
4. The method for preparing a multilayer high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating according to claim 3, characterized in that: In step S2 and step S3, the solution-aging treatment is specifically The following steps are involved: A1. Place AlCoCrNiMo alloy powder or AlCoCrNiMoBSi alloy powder in a vacuum heat treatment furnace, close the furnace cover, and evacuate the interior of the vacuum heat treatment furnace to 10 -5 Below Pa; A2, vacuum to 10 -5 After the temperature reaches 1150°C at a heating rate of 10°C / min, the temperature is kept at this temperature for 5 hours, and the AlCoCrNiMo alloy powder or the AlCoCrNiMoBSi alloy powder is subjected to a solid solution treatment at a solid solution treatment temperature of 1150°C and a solid solution treatment time of 5 hours; A3, after the solution treatment, the temperature is lowered to 600°C and kept at this temperature for 4 hours, and the AlCoCrNiMo alloy powder or AlCoCrNiMoBSi alloy powder is subjected to aging treatment at a temperature of 600°C and a aging treatment time of 4 hours; A4, after the aging treatment is completed, the vacuum degree inside the furnace chamber is maintained, and the furnace is cooled to room temperature, and finally AlCoCrNiMo high entropy alloy powder or AlCoCrNiMoBSi high entropy alloy powder is obtained.
5. The method for preparing a multilayer high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating according to claim 4, characterized in that: In the step A1, the preparation method of the AlCoCrNiMo alloy powder is as follows: first, the single substance Cr and Mo powders are ball-milled for 25 hours, then the single substance Co powder is added and ball-milled for 35 hours, and then the single substance Al and Ni powders are added and ball-milled for 45 hours; the molar ratio of the single substance powder elements of the AlCoCrNiMo alloy powder is Al:Co:Cr:Ni:Mo=1:1:1:1:1, and the particle size of the single substance Al, Co, Cr, Ni, and Mo powders is 15-45 μm.
6. The method for preparing a multilayer high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating according to claim 4, characterized in that: In the step A1, the preparation method of AlCoCrNiMoBSi alloy powder is as follows: first, ball-mill the single-substance Cr and Mo powders for 25 hours, then add the single-substance Co powder and ball-mill for 35 hours, add the single-substance Al and Ni powders and ball-mill for 45 hours, and then add the single-substance B and Si powders and ball-mill for 55 hours; the single-substance powder molar ratio of the AlCoCrNiMoBSi alloy powder is Al:Co:Cr:Ni:Mo:B:Si=1:1:1:1:1:0.1:0.15, the particle size of the single-substance Al, Co, Cr, Ni, and Mo powders is 15-45μm, and the particle size of the single-substance B and Si powders is 1-3μm.
7. The method for preparing a multilayer high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating according to claim 3, characterized in that: In step S2, the oxygen-kerosene supersonic flame spraying process parameters are as follows: kerosene flow rate is 26m 3 / h, oxygen flow rate is 53m 3 / h, spraying distance is 380mm, spraying step is 3mm, spray gun moving speed is 800mm / s, barrel size is 6inch, powder feeding rate is 50g / min, spraying 2~3 times.
8. The method for preparing a multi-layer structured high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating as claimed in claim 3, characterized in that: In step S3, the oxygen-kerosene supersonic flame spraying process parameters are as follows: kerosene flow rate is 32m 3 / h, oxygen flow rate is 53m 3 / h, spraying distance is 380mm, spraying step is 3mm, spray gun moving speed is 800mm / s, barrel size is 6inch, powder feeding rate is 50g / min, spraying 3~5 times.
9. The method for preparing a multi-layer structured high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating as claimed in claim 3, characterized in that: In step S4, the oxygen-kerosene supersonic flame spraying process parameters are as follows: kerosene flow rate is 32m 3 / h, oxygen flow rate is 53m 3 / h, spraying distance is 380mm, spraying step is 3mm, spray gun moving speed is 800mm / s, barrel size is 6inch, powder feeding rate is 50g / min, spraying is 8~15 times.
10. The method for preparing a multi-layer structured high thermal conductivity, wear resistance, heat resistance and corrosion resistance high entropy alloy coating according to claim 3, characterized in that: In step S4, the specific steps of nitriding treatment are as follows: B1, put the sample to be nitrided into the nitriding furnace and seal the furnace body; before formal nitriding, pump the nitriding furnace to below 5Pa; B2, heating stage: when the nitriding furnace reaches the predetermined vacuum degree, adjust the nitrogen / hydrogen flow rate to make the pressure value in the furnace 60-80Pa, increase the power supply voltage to 450V, and introduce nitrogen / hydrogen flow at the same time. According to the arc state inside the nitriding furnace, slowly adjust the voltage and conduction ratio to make the temperature in the furnace rise and maintain a stable glow. When the temperature reaches 300℃, turn on the furnace cooling water to cool the furnace wall until the temperature reaches the preset temperature of 600℃; B3, insulation stage: when the nitriding furnace reaches the preset temperature, the control voltage is 720V, the nitrogen flow rate is 600sccm, the hydrogen flow rate is 200sccm, and the duty cycle is 3:1 to ensure the stability of the temperature and pressure in the furnace. The insulation stage lasts for 8~48h; B4, cooling stage: After the insulation is completed, turn off the power and continue to introduce nitrogen / hydrogen with a nitrogen flow rate of 600sccm and a hydrogen flow rate of 200sccm to maintain a reducing atmosphere in the nitriding furnace to prevent oxidation. Cool with the furnace to finally obtain a multi-layer structure of a high thermal conductivity, wear-resistant, heat-resistant and corrosion-resistant high-entropy alloy coating.
Citation Information
Patent Citations
Method for preparing high-entropy alloy coatings through magnetron sputtering
CN109402590A
Method for preventing internal oxidation of high-entropy alloy coating containing Cr and Al by adding Si
CN112853347A
Preparation method of high-entropy alloy nitride coating metallurgically bonded with matrix
CN113652659A
Nickel-based high-temperature alloy material and preparation method thereof
CN114293147A
Pot and cooking equipment
CN114642363A
Cited By
Ceramic coating and preparation method thereof
CN121228153A