High-strength anti-crack concrete and preparation method thereof
By synergistically modifying tannin and starch under acidic conditions and optimizing the fiber ratio, the problem of decreasing crack resistance of tanninic acid-modified concrete in high-temperature drying environments is solved, and the effect of significantly improving compressive strength and crack resistance is achieved.
Patent Information
- Application Number
- CN202510297476.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-13
- Publication Date
- 2025-06-13
Smart Images

Figure CN120136500A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of concrete technology and relates to a high-strength crack-resistant concrete and a preparation method thereof. Background Art
[0002] As the most widely used building material globally, concrete has long been restricted in its reliability in complex environments due to its large brittleness, low tensile strength, and easy cracking. Especially in projects such as bridges, roads, and high-rise buildings, the crack problems in concrete caused by temperature changes, shrinkage stress, or external loads not only reduce the structural durability but may also pose safety hazards. To overcome this bottleneck, fiber reinforcement technology has been widely introduced into the field of concrete modification. By incorporating steel fibers, synthetic fibers, or natural fibers, the crack resistance and toughness of concrete can be effectively improved. The reinforcement mechanism of fibers mainly relies on their bridging effect in the matrix, that is, the fibers span the crack area and delay the crack propagation and disperse the stress concentration through the interfacial bonding force. At the same time, the fiber network can restrain the early plastic shrinkage and drying shrinkage of concrete and reduce the generation of microcracks. However, the interfacial compatibility between fibers and the concrete matrix has become a key factor restricting the improvement of its performance. If there are problems such as high porosity, weak chemical bonding, or poor physical stability in the interfacial transition zone (ITZ), the fibers are prone to slip or debond, resulting in a significant decrease in the reinforcement efficiency and even becoming the origin point of cracks.
[0003] Regarding the optimization of the fiber-concrete interface, researchers have proposed various surface modification methods, including chemical etching, coupling agent modification, and natural substance coating. In recent years, tannic acid, as a natural polyphenol compound, has received attention due to its environmental friendliness, low cost, and versatility. Tannic acid can form hydrogen bonds or covalent bonds with the surface groups of fibers (such as the hydroxyl groups of cellulose fibers or the oxygen-containing groups of synthetic fibers) through phenolic hydroxyl groups, and at the same time, chelate with calcium ions in the cement hydration products to construct a stable chemical bridging structure between the fibers and the matrix. This process not only enhances the interfacial bonding strength but also fills the micro-pores in the interfacial area and improves the density. In addition, the antioxidant properties of tannic acid can delay the oxidative degradation of fibers in an alkaline environment, thus maintaining long-term interfacial stability. For example, CN114315197A discloses a fiber concrete interface modifier and a modification method. The raw materials of the fiber concrete interface modifier include water and tannic acid, wherein the mass fraction of tannic acid is ≥1%, the pH of the fiber concrete interface modifier is between 3 and 6, and the fiber concrete interface modification method is to treat the fibers with the fiber concrete interface modifier and then mix the treated fibers with the concrete. This invention can effectively improve the chemical bonding strength between the fibers and the concrete, improve the durability of the fibers, improve the dispersion of the fibers in the concrete, improve the deformation ability of the fiber concrete, increase the total energy absorption when the fiber concrete fails, and greatly enhance the mechanical and durable properties of the fiber concrete.
[0004] However, the above modification system exhibits obvious performance degradation in the high-temperature and dry outdoor environment. The synergistic effect of high temperature and low humidity leads to a significant decline in the crack resistance of tannic acid-modified concrete, specifically manifested as surface cracking, deep crack propagation, and large-area debonding between fibers and the matrix. The occurrence of this phenomenon is closely related to the physicochemical properties of tannic acid and the environmental action mechanism. First of all, tannic acid has low thermal stability and is prone to oxidation under continuous high temperature, generating small molecule carboxylic acids and phenolic fragments, and the original chemical bridging structure is destroyed accordingly, resulting in a sharp decline in the interfacial bonding strength. Secondly, high temperature accelerates the evaporation of internal water in concrete, and tannic acid is prone to generate microcracks due to shrinkage during this process, which further increases the matrix porosity and forms connected defect channels. The unevenness of water migration leads to the concentration of shrinkage stress, promoting the development of microcracks into macro cracks. In addition, the retarding effect of tannic acid on cement hydration is amplified in the high-temperature environment, resulting in a lag in the early strength development of concrete, and the rapid loss of surface water forms a "hard outside and soft inside" gradient structure, exacerbating the cracking risk caused by the imbalance between internal and external stresses. More critically, in the high-temperature and dry environment, the elastic modulus of the interfacial region between concrete and fibers decreases, and tannic acid cannot coordinate the difference in thermal expansion coefficients between fibers and the concrete matrix, ultimately leading to fiber debonding failure and accelerated crack propagation.
[0005] Although the prior art has improved the crack resistance of fiber concrete through tannic acid modification in the conventional environment, its limitations in the high-temperature and dry environment have not been effectively solved. Specifically, it is manifested as insufficient thermal stability of the modifier, lack of control means for the deterioration of thermal-mechanical coupling at the interface, and the dynamic influence of environmental humidity fluctuations on chemical bonding has not been fully considered. This technical bottleneck severely restricts the popularization and application of such materials in desert, arid regions, or high-temperature industrial environments. Therefore, developing a fiber concrete modification technology that adapts to extreme environments and takes into account interface enhancement and long-term stability has become a key issue that urgently needs to be broken through in the field of building materials. Summary of the Invention
[0006] The purpose of the present invention is to solve the technical problem that using tannic acid to improve the strength of basic concrete will lead to a decline in its crack resistance in the high-temperature and dry environment. In this regard, the present invention provides a high-strength crack-resistant concrete and its preparation method to solve this need in the art.
[0007] On the one hand, the present invention relates to a preparation method of concrete, which includes: making a modifier by mixing tannic acid, starch, and water;
[0008] immersing fibers in the modifier for modification to obtain modified fibers, and mixing the modified fibers and basic concrete to obtain the concrete;
[0009] The basic concrete includes ordinary Portland cement, coarse aggregate, fine aggregate, and water.
[0010] Furthermore, in the concrete preparation method provided by the present invention, the pH of the modifier is 3 to 5.
[0011] Furthermore, in the concrete preparation method provided by the present invention, by mass percentage, in the modifier, the content of tannic acid is 1 to 10%, and the content of starch is 4 to 12%.
[0012] Furthermore, in the concrete preparation method provided by the present invention, by weight, the raw materials include: 100 parts of ordinary Portland cement, 200 - 300 parts of coarse aggregate, 100 - 150 parts of fine aggregate, 30 - 50 parts of water, and 10 - 30 parts of the modified fiber.
[0013] Furthermore, in the concrete preparation method provided by the present invention, the modification time is 30 - 120 min.
[0014] Furthermore, in the concrete preparation method provided by the present invention, the fiber is selected from at least one of basalt fiber, carbon fiber, and steel fiber.
[0015] Furthermore, in the concrete preparation method provided by the present invention, the fiber is composed of basalt fiber and steel fiber.
[0016] Furthermore, in the concrete preparation method provided by the present invention, the mass ratio of basalt fiber to steel fiber is 1:90 - 100.
[0017] Furthermore, in the concrete preparation method provided by the present invention, the length of the basalt fiber is 5 - 10 mm, and the length of the steel fiber is 30 - 50 mm.
[0018] On the other hand, the present invention relates to a concrete prepared by using the above-mentioned concrete preparation method.
[0019] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages:
[0020] Through the synergistic modification of tannic acid and starch under acidic conditions, the optimization of the composite ratio of basalt fiber and steel fiber, and the precise control of process parameters, the present invention significantly surpasses the limitations of the prior art. In an extreme environment of high temperature and dryness, the compressive strength of Example 6 reaches 66 MPa, the initial cracking time is extended to 48 minutes, and the maximum crack length is only 41 mm. Compared with the traditional tannic acid modification system, its crack resistance is improved by more than 70%, and the strength increase is 50%. The introduction of starch not only inhibits the thermal oxidation failure of tannic acid through the viscoelastic network, but also fills the interfacial pores to reduce shrinkage stress. The tannic acid-starch complex formed under acidic conditions strengthens the chemical bonding and physical anchoring between the fiber and the matrix, solving the interfacial deterioration problem that has long troubled tannic acid-modified concrete. Basalt fiber and steel fiber are compounded at a mass ratio of 1:90 to 1:100. Through the synergistic mechanism of short fibers blocking microcracks and long fibers bridging macro-cracks, "micro-macro" dual-scale crack resistance is achieved. The addition of starch as a low-cost natural raw material, combined with the acidic modification process that does not require complex equipment, further reduces the threshold of industrial application. While maintaining high strength, the present invention overcomes the crack resistance defects caused by the thermal oxidation failure of tannic acid and the insufficient design of the fiber system in traditional technologies, providing a concrete solution with durability, environmental adaptability and economy for projects such as bridges and high-rise buildings in high-temperature and arid regions. Description of the Drawings
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following will briefly introduce the drawings required for the description of the embodiments or the prior art. Obviously, the following drawings are only some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can be obtained based on these drawings.
[0022] Figure 1 The test block prepared in Example 3.
[0023] Figure 2 The test block prepared in Comparative Example 1. Detailed Embodiments
[0024] Next, the technical solutions of the present invention will be described in conjunction with the embodiments. However, the present invention is not limited to the following embodiments. The experimental methods and detection methods described in each embodiment are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified. The %, as used in the following embodiments, is the mass percentage unless otherwise specified. The ratios in the following embodiments are mass ratios unless otherwise specified.
[0025] Example 1
[0026] This example provides a preparation process of concrete.
[0027] The raw materials used include: tannic acid (purity > 99%), starch (corn starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), basalt fiber (diameter of 11 μm and length of 5 mm), water reducing agent (polycarboxylate water reducing agent) and water.
[0028] Step 1: Mix tannic acid, starch and water and then ultrasonicate (power: 400 W, time: 30 min) to make the texture uniform, and then add the pH regulator to control the pH of the mixture to 3 to obtain the modified liquid. The content of tannic acid in the modifier is 1%, and the content of starch is 4%.
[0029] Step 2: Immerse the basalt fiber into the modified liquid prepared in Step 1 for modification. By mass ratio, the mass ratio of the fiber to the modified liquid is 1:10. After ultrasonication (power: 400 W, time: 30 min) at room temperature, take it out to obtain the modified fiber.
[0030] Step 3: By weight, take 100 parts of ordinary Portland cement, 200 parts of coarse aggregate, 100 parts of fine aggregate, 30 parts of water, 10 parts of modified fiber and 1 part of water reducing agent; first mix the fine aggregate, coarse aggregate and cement evenly, then add water and the water reducing agent and stir evenly to obtain the premix; finally, put the modified fiber into the premix and mix evenly to obtain the Figure 1 concrete test block as shown.
[0031] Example 2
[0032] This example provides a preparation process of concrete.
[0033] The raw materials used include: tannic acid (purity > 99%), starch (sweet potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), carbon fiber (diameter of 8 μm and length of 6 mm), water reducing agent (polycarboxylate water reducing agent) and water.
[0034] Step 1: Mix tannic acid, starch and water and then ultrasonicate (power: 400 W, time: 30 min) to make the texture uniform, and then add the pH regulator to control the pH of the mixture to 4 to obtain the modified liquid. The content of tannic acid in the modifier is 5%, and the content of starch is 8%.
[0035] Step 2: Immerse the carbon fiber into the modifier prepared in Step 1 for modification. By mass ratio, the mass ratio of the fiber to the modification liquid is 1:10. After ultrasonic treatment (power: 400 W, time: 60 min) at room temperature, take it out to obtain the modified fiber.
[0036] Step 3: By weight, take 100 parts of ordinary Portland cement, 250 parts of coarse aggregate, 120 parts of fine aggregate, 40 parts of water, 20 parts of modified fiber, and 1 part of water reducing agent; first stir the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducing agent and stir evenly to obtain a premix; finally, put the modified fiber into the premix and mix evenly to obtain it.
[0037] Example 3
[0038] This example provides a preparation process of concrete.
[0039] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), steel fiber (diameter: 0.5 mm, length: 30 mm), water reducing agent (polycarboxylate water reducing agent), and water.
[0040] Step 1: Mix tannic acid, starch, and water and perform ultrasonic treatment (power: 400 W, time: 30 min) to make its texture uniform, then add the pH regulator to control the pH of the mixed solution to 4 to obtain the modification liquid. The content of tannic acid in the modifier is 10%, and the content of starch is 12%.
[0041] Step 2: Immerse the steel fiber into the modifier prepared in Step 1 for modification. By mass ratio, the mass ratio of the fiber to the modification liquid is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take it out to obtain the modified fiber.
[0042] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fiber, and 1 part of water reducing agent; first stir the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducing agent and stir evenly to obtain a premix; finally, put the modified fiber into the premix and mix evenly to obtain it.
[0043] Example 4
[0044] This example provides a preparation process of concrete.
[0045] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), basalt fiber (diameter of 11 μm and length of 5 mm), steel fiber (diameter of 0.5 mm and length of 30 mm), water reducing agent (polycarboxylate water reducing agent) and water.
[0046] Step 1: Mix tannic acid, starch and water, and then ultrasonically treat them (power: 400 W, time: 30 min) to make the texture uniform. Then add the pH regulator to control the pH of the mixed solution to 4 to obtain the modified solution. The content of tannic acid in the modifier is 10%, and the content of starch is 12%.
[0047] Step 2: Mix basalt fiber and steel fiber at a mass ratio of 1:90, immerse them in the modified agent prepared in Step 1 for modification. By mass, the mass ratio of the fiber to the modified solution is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take them out to obtain the modified fiber.
[0048] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fiber and 1 part of water reducing agent; first stir the fine aggregate, coarse aggregate and cement evenly, then add water and water reducing agent and stir evenly to obtain the premix; finally, put the modified fiber into the premix and mix evenly to obtain it.
[0049] Example 5
[0050] This example provides a preparation process of concrete.
[0051] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), basalt fiber (diameter of 11 μm and length of 5 mm), steel fiber (diameter of 0.5 mm and length of 30 mm), water reducing agent (polycarboxylate water reducing agent) and water.
[0052] Step 1: Mix tannic acid, starch and water, and then ultrasonically treat them (power: 400 W, time: 30 min) to make the texture uniform. Then add the pH regulator to control the pH of the mixed solution to 4 to obtain the modified solution. The content of tannic acid in the modifier is 10%, and the content of starch is 12%.
[0053] Step 2: Mix basalt fibers and steel fibers at a mass ratio of 1:95, then immerse them in the modifier prepared in Step 1 for modification. By mass, the mass ratio of the fibers to the modifier solution is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take them out to obtain modified fibers.
[0054] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fibers, and 1 part of water reducing agent; first mix the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducing agent and mix evenly to obtain a premix; finally, put the modified fibers into the premix and mix evenly to obtain the product.
[0055] Example 6
[0056] This example provides a preparation process of concrete.
[0057] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), basalt fibers (diameter: 11 μm, length: 5 mm), steel fibers (diameter: 0.5 mm, length: 30 mm), water reducing agent (polycarboxylate water reducing agent), and water.
[0058] Step 1: Mix tannic acid, starch, and water, then perform ultrasonic treatment (power: 400 W, time: 30 min) to make the texture uniform, and then add the pH regulator to control the pH of the mixed solution to 4 to obtain a modifier. The content of tannic acid in the modifier is 10%, and the content of starch is 12%.
[0059] Step 2: Mix basalt fibers and steel fibers at a mass ratio of 1:100, then immerse them in the modifier prepared in Step 1 for modification. By mass, the mass ratio of the fibers to the modifier solution is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take them out to obtain modified fibers.
[0060] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fibers, and 1 part of water reducing agent; first mix the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducing agent and mix evenly to obtain a premix; finally, put the modified fibers into the premix and mix evenly to obtain the product.
[0061] Comparative Example 1
[0062] This comparative example provides a preparation process of concrete modified with ordinary tannic acid.
[0063] The raw materials used include: tannic acid (purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), steel fiber (with a diameter of 0.5 mm and a length of 30 mm), water reducing agent (polycarboxylate water reducing agent), and water.
[0064] Step 1: Mix tannic acid and water and then ultrasonicate (power: 400 W, time: 30 min) to make the texture uniform, and then add the pH regulator to control the pH of the mixture to 4 to obtain the modified liquid. The content of tannic acid in the modifier is 22%.
[0065] Step 2: Immerse the steel fiber in the modifier prepared in Step 1 for modification. By mass ratio, the mass ratio of the fiber to the modified liquid is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take it out to obtain the modified fiber.
[0066] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fiber, and 1 part of water reducing agent; first mix the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducing agent and stir evenly to obtain the premix; finally, put the modified fiber into the premix and mix evenly to obtain the Figure 2 test block as shown.
[0067] Comparative Example 2
[0068] This comparative example provides the preparation process of concrete with starch directly incorporated.
[0069] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), steel fiber (with a diameter of 0.5 mm and a length of 30 mm), water reducing agent (polycarboxylate water reducing agent), and water.
[0070] Step 1: Mix tannic acid and water and then ultrasonicate (power: 400 W, time: 30 min) to make the texture uniform, and then add the pH regulator to control the pH of the mixture to 4 to obtain the modified liquid. The content of tannic acid in the modifier is 10%.
[0071] Step 2: Immerse the steel fibers in the modifier prepared in Step 1 for modification. By mass ratio, the mass ratio of the fibers to the modification liquid is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take them out to obtain modified fibers.
[0072] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fibers, 1 part of water reducer, and 5 parts of starch; first, stir the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducer and stir evenly to obtain a premix; finally, put the modified fibers into the premix and mix evenly to obtain the product.
[0073] Comparative Example 3
[0074] This comparative example provides the preparation process of concrete.
[0075] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), basalt fiber (diameter: 17 μm, length: 19 mm), steel fiber (diameter: 0.5 mm, length: 30 mm), water reducer (polycarboxylate water reducer), and water.
[0076] Step 1: Mix tannic acid, starch, and water and perform ultrasonic treatment (power: 400 W, time: 30 min) to make their texture uniform, then add the pH regulator to control the pH of the mixed solution to 4 to obtain a modification liquid. The content of tannic acid in the modifier is 10%, and the content of starch is 12%.
[0077] Step 2: Mix basalt fibers and steel fibers at a mass ratio of 1:100, immerse them in the modifier prepared in Step 1 for modification. By mass ratio, the mass ratio of the fibers to the modification liquid is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take them out to obtain modified fibers.
[0078] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fibers, and 1 part of water reducer; first, stir the fine aggregate, coarse aggregate, and cement evenly, then add water and the water reducer and stir evenly to obtain a premix; finally, put the modified fibers into the premix and mix evenly to obtain the product.
[0079] Comparative Example 4
[0080] This comparative example provides the preparation process of concrete.
[0081] The raw materials used include: tannic acid (purity > 99%), starch (potato starch, purity > 99%), ordinary Portland cement (P.O 42.5), coarse aggregate (crushed stone with an average particle size of 10 mm), fine aggregate (natural sand with a particle size less than 5 mm and a fineness modulus of 2.6 - 3.0), pH regulator (0.1 moL / L NaOH aqueous solution), basalt fiber (diameter of 11 μm and length of 5 mm), steel fiber (diameter of 0.5 mm and length of 30 mm), water reducing agent (polycarboxylate water reducing agent), and water.
[0082] Step 1: Mix tannic acid, starch, and water, and then ultrasonicate (power: 400 W, time: 30 min) to make the texture uniform. Then add a pH regulator to control the pH of the mixed solution to 4 to obtain a modified solution. The content of tannic acid in the modifier is 10%, and the content of starch is 12%.
[0083] Step 2: Mix basalt fiber and steel fiber in a mass ratio of 1:1, immerse them in the modified agent prepared in Step 1 for modification. By mass, the mass ratio of the fiber to the modified solution is 1:10. After ultrasonic treatment (power: 400 W, time: 120 min) at room temperature, take them out to obtain modified fibers.
[0084] Step 3: By weight, take 100 parts of ordinary Portland cement, 300 parts of coarse aggregate, 150 parts of fine aggregate, 50 parts of water, 30 parts of modified fiber, and 1 part of water reducing agent; first, stir the fine aggregate, coarse aggregate, and cement evenly, then add water and water reducing agent, and stir evenly to obtain a premix; finally, put the modified fiber into the premix and mix evenly to obtain the product.
[0085] Test Example
[0086] This test example provides the performance test results of Examples 1 - 6 and Comparative Examples 1 - 4.
[0087] Compressive strength test: The size of the specimen is 100 mm × 100 mm × 100 mm. Each group is designed with 3 specimens, a total of 15 groups. Demold after 24 h of casting and molding, move them to the curing room, set the ambient temperature to 35 ± 2 °C, and the ambient relative humidity not greater than 30 ± 5%. After curing for 28 d, conduct compressive strength testing at 0.6 MPa / s.
[0088] Anti-cracking performance test: Refer to "Anti-cracking and anti-seepage composite materials for concrete" (T / CECS 10001—2019) to conduct the early anti-cracking performance test. Use a steel mold with dimensions of 600mm×600mm×200mm, and a crack inducer is installed inside. After the large plate is cast and formed, the accelerated cracking test is started. Use a floodlight for irradiation and an electric fan for air drying to control the wind direction parallel to the surface of the specimen. The wind speed in the middle of the specimen surface is not less than 4m / s, the ambient temperature is 35±2°C, and the ambient relative humidity is not more than 30±5%. Record the initial cracking time and the maximum crack length.
[0089] The test results are shown in Table 1.
[0090] Table 1: Compressive strength and anti-cracking performance of concrete
[0091]
[0092] Based on the test results in Table 1, it can be seen from Comparative Example 1 and Comparative Example 2 that by introducing an acidic condition in the present invention, the degree of protonation of the phenolic hydroxyl groups of tannic acid is increased, and the intermolecular hydrogen bonds are enhanced, which promotes the formation of a stable complex with starch molecules through hydrogen bonds and hydrophobic interactions. The colloidal properties of starch are significantly improved in this environment, forming a viscoelastic network structure, which not only uniformly disperses tannic acid but also anchors it on the fiber surface through physical adsorption. This complex not only retains the chemical bonding ability of tannic acid with the functional groups (such as hydroxyl groups and metal oxides) on the fiber surface but also reduces the porosity of the interfacial region through the filling effect of starch, thereby inhibiting the initiation of microcracks and further optimizing the modification effect of the fiber-concrete interface, resulting in high-strength anti-cracking concrete and better solving the technical problem that using tannic acid to improve the strength of basic concrete will lead to a decrease in its anti-cracking ability in high-temperature and dry environments. It can be seen from Examples 4 to 6 and Comparative Examples 3 to 4 that by controlling the fiber ratio and length and combining the synergistic effect of the tannic acid-starch acidic modifier, efficient interfacial strengthening and stress dispersion of the fiber composite system are achieved. However, in Comparative Examples 3 to 4, due to the imbalance of the fiber ratio or the excessive length, the interfacial defects increase, verifying the necessity of optimizing the fiber system. This design not only improves the compressive strength and anti-cracking property of concrete but also maintains the interfacial stability in extreme environments, providing a reliable solution for engineering applications.
[0093] As described above, the basic principle, main features, and advantages of the present invention are preferably described. The above embodiments and the description are only descriptions of the preferred embodiments of the present invention. The present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by those of ordinary skill in the art to the technical solutions of the present invention shall fall within the protection scope determined by the present invention.
Claims
1. A method for preparing concrete, characterized in that: include: A modifying agent is prepared by preparing tannic acid, starch and water; The fiber is immersed in the modifier for modification to obtain modified fiber, and the modified fiber is mixed with base concrete to obtain the concrete; The base concrete includes ordinary Portland cement, coarse aggregate, fine aggregate and water.
2. The method for preparing concrete according to claim 1, characterized in that: The pH of the modifier is 3-5.
3. The method for preparing concrete according to claim 1, characterized in that: In terms of mass percentage, in the modifier, the content of tannic acid is 1-10%, and the content of starch is 4-12%.
4. The method for preparing concrete according to claim 1, characterized in that: The raw materials include, by weight, 100 parts of ordinary Portland cement, 200-300 parts of coarse aggregate, 100-150 parts of fine aggregate, 30-50 parts of water and 10-30 parts of the modified fiber.
5. The method for preparing concrete according to claim 1, characterized in that: The modification time is 30 to 120 minutes.
6. The method for preparing concrete according to claim 1, characterized in that: The fiber is selected from at least one of basalt fiber, carbon fiber and steel fiber.
7. The method for preparing concrete according to claim 6, characterized in that: The fibers are composed of basalt fibers and steel fibers.
8. The method for preparing concrete according to claim 7, characterized in that: The mass ratio of basalt fiber to steel fiber is 1:90-100.
9. The method for preparing concrete according to claim 1, characterized in that: The length of the basalt fiber is 5 to 10 mm, and the length of the steel fiber is 30 to 50 mm.
10. A concrete, characterized in that: The concrete is prepared by the method for preparing concrete according to any one of claims 1 to 9.
Citation Information
Patent Citations
Fiber concrete interface modifier and modification method
CN114315197A
Cited By
Modified asphalt concrete used in high temperature-cold shock environment and preparation method thereof
CN121181287A
Modified asphalt concrete for high temperature-cold impact environment and method for preparing the same
CN121181287B