Method for recovering barite from solid discharged from drilling solid control system

By using acid oxidant solution and dispersant in the solid discharged from the drilling solid control system for pretreatment, combined with flotation technology, the recycling quality and suitability of barite have been successfully improved, and the problems of low quality and high treatment cost in the prior art have been solved.

CN120155304APending Publication Date: 2025-06-17CHINA NAT PETROLEUM CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311716921.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2025-06-17

AI Technical Summary

Technical Problem

The existing barite recycling technology has problems such as low quality, high processing cost and unsuitable for industrial applications.

Method used

The solid discharged from the drilling solid control system is mixed with water and slurry, and the acid oxidant solution and dispersant are added for pretreatment, followed by flotation to purify the barite. The method includes multiple slurry processing steps, through the acidification and oxidation of the acid oxidant solution, the dispersion of the dispersant, improve the flotation efficiency and improve the quality of barite.

Benefits of technology

It realizes the recycling of high-quality barite, reduces processing costs, simplifies equipment demand, is suitable for industrial applications, and reduces energy consumption and equipment costs through room temperature treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120155304A_ABST
    Figure CN120155304A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recovering barite from solids discharged from a well drilling solid control system, which comprises the following steps: mixing the solids discharged from the well drilling solid control system with water to obtain first slurry; an acidic oxidant solution and the first slurry are mixed and stirred, solid-liquid separation is carried out, an obtained solid phase part is mixed with water for slurry mixing, and second slurry is obtained; a dispersing agent and the second slurry are mixed and stirred, solid-liquid separation is carried out, an obtained solid phase part is mixed with water, slurry mixing is carried out, and third slurry is obtained; mixing and stirring a flotation agent and the third slurry, and then carrying out flotation to obtain barite. The barite recycled by the method is high in quality and beneficial to quality control and medicament saving, the whole treatment process is normal-temperature treatment, calcination is not needed, equipment simplification is facilitated, and energy consumption and equipment cost are reduced. And the required treatment equipment is simple and is easy to compact and integrate for use, so that industrial production and application are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of oil and gas drilling, and particularly relates to a method for recovering barite from solids discharged from a drilling solids control system. Background Art

[0002] During the oil and gas drilling process, drilling fluid is used to carry drill cuttings, balance formation pressure, lubricate drill tools, etc. The drilling fluid is composed of various components such as water, bentonite, drilling fluid additives, and weighting materials. Barite is a commonly used weighting material for drilling fluid. In high-density drilling fluid, the addition amount of barite can even be as high as more than 60%. Therefore, the annual consumption of barite in the world is huge. During the cyclic application process of the drilling fluid, it is often necessary to discharge solids, and part of the barite is discharged and discarded, which not only causes waste of resources but also increases the production of drilling solid waste. Recycling and reuse are beneficial to the comprehensive utilization of resources and environmental protection.

[0003] However, in the solids discharged from the drilling solids control system, in addition to barite (barium sulfate), it also contains carbonates (such as dolomite, calcite), silicates (such as clay minerals, quartz), and a large amount of organic additives (such as partially hydrolyzed polyacrylamide PHP, sulfonated phenolic resin SMP, sulfonated tannin SMT, lignosulfonate, sulfonated asphalt SAS, etc.). Due to the small size of various solid-phase particles, it is difficult to effectively separate barite by simply using conventional methods such as gravity separation, centrifugal separation, and hydrocyclone separation. In theory, flotation can be used to separate barite, but due to the high content of organic components in the solids discharged from the drilling solids control system, the flotation separation effect is seriously affected.

[0004] CN115676868A discloses a method for recovering barium sulfate from solid waste containing barium salt mud: adding hydrochloric acid to dissolve and filter, neutralizing the filtrate with ammonia water and then reacting with sulfuric acid to separate and obtain precipitated barium sulfate. After washing the filter residue, it is successively calcined and reacted with carbon powder at high temperature, dissolved and filtered with hydrochloric acid, and the washing solution is reacted with sulfuric acid to obtain precipitated barium sulfate. The calcination temperature is as high as 600 - 800°C, the consumption of hydrochloric acid and sulfuric acid is large, and high-temperature calcination equipment is required, resulting in high treatment costs.

[0005] CN104609455B discloses a method for recovering barite from waste drilling mud. By adding sulfuric acid and water treatment, then adding a flotation agent and using a flotation machine to recover barite, and finally using a barite modifier for modification treatment, barite that can be used for weighting drilling fluid is obtained. The process of this patent has a long treatment time and low efficiency.

[0006] CN116060205A discloses a process for recovering barite from the remaining solid phase after thermal desorption of drilling oil-based cuttings: the remaining solid phase is screened, slurried with water, and then floated by the nano-bubble reverse flotation method. The scraped scum is then centrifuged to recover barite. This patent targets the remaining solid phase after thermal desorption treatment, and almost all the organic matter affecting flotation has been completely removed, and it is not applicable to the cuttings directly discharged from the drilling solids control system.

[0007] Therefore, there are defects in the existing barite recovery, such as low quality, high recovery and treatment cost, and inapplicability to industrial applications, which have become technical problems to be solved urgently. Summary of the Invention

[0008] In view of the deficiencies of the existing technology, the present invention provides a method for recovering barite from the solids discharged from the drilling solids control system with high barite recovery quality, low recovery and treatment cost, and suitable for industrial applications.

[0009] The present invention provides a method for recovering barite from the solids discharged from the drilling solids control system, including: mixing the solids discharged from the drilling solids control system with water to form a first slurry; mixing an acidic oxidant solution with the first slurry and stirring, followed by solid-liquid separation, and mixing the obtained solid phase portion with water to form a second slurry; mixing a dispersant with the second slurry and stirring, followed by solid-liquid separation, and mixing the obtained solid phase portion with water to form a third slurry; mixing a flotation agent with the third slurry and stirring, and then performing flotation to obtain barite.

[0010] According to a specific embodiment of the present invention, the solid content in the first slurry is less than 20% v / v.

[0011] According to a specific embodiment of the present invention, the acidic oxidant solution is a mixed solution of an acid and an oxidant, and the oxidant is selected from any one of sodium hypochlorite, calcium hypochlorite, and hydrogen peroxide, and the acid is selected from any one of hydrochloric acid, sulfuric acid, oxalic acid, and acetic acid.

[0012] According to a specific embodiment of the present invention, in the acidic oxidant solution, the molar ratio of the oxidant to the acid is 1:2 to 5.

[0013] According to a specific embodiment of the present invention, the addition amount of the acidic oxidant solution is adjusted so that the pH value of the mixed liquid of the acidic oxidant solution and the first slurry is 4 to 6.

[0014] According to a specific embodiment of the present invention, the solid content of the second slurry is 5% to 20% v / v.

[0015] According to a specific embodiment of the present invention, the dispersant is selected from any one of sodium hydroxide solution, water glass solution, and sodium hexametaphosphate solution.

[0016] According to a specific embodiment of the present invention, the addition amount of the dispersant is adjusted so that the pH of the mixed liquid of the dispersant and the second slurry is 9-10.

[0017] According to a specific embodiment of the present invention, the solid content of the third slurry is 5%-20% v / v.

[0018] According to a specific embodiment of the present invention, the method of solid-liquid separation includes separation using a settling tank or a hydrocyclone separator.

[0019] According to a specific embodiment of the present invention, the flotation agent is sodium dodecyl sulfate; preferably, the addition amount of the flotation agent is 50-200 mg / L.

[0020] According to a specific embodiment of the present invention, it further includes washing the barite obtained by flotation; preferably, it is washed with a mixed solution of hydroxyl paraffin oil and water.

[0021] According to a specific embodiment of the present invention, it further includes recovering the water in the waste liquid generated in each step for recycling.

[0022] According to a specific embodiment of the present invention, the recovery method is: first adjust the pH value of the waste liquid to 6.5-7.0, then perform coagulation treatment with a polyaluminum chloride solution and a polyacrylamide solution, and after completion, centrifuge to separate and discard the slag to obtain it.

[0023] The beneficial effects of the present invention are:

[0024] The present invention particularly adopts a method of first pretreating with an acidic oxidant solution and a dispersant, and then performing flotation to purify barite. Among them, the acidic oxidant solution has both acidification and oxidation effects. During the process of acidifying and decomposing impurity components such as carbonate rocks and silicate rocks, it can simultaneously oxidize and erode the organic additives on the surface of barite particles; the dispersant is beneficial to improving the dispersibility of impurity components and inhibiting the influence of clay minerals on dispersion. Through the combined action of the above two aspects, the subsequent flotation treatment efficiency is greatly improved, and the quality of the recovered barite is improved. The method of the present invention is beneficial to quality control and saves chemicals. The entire treatment process is at room temperature and does not require calcination, which is convenient for simplifying equipment, reducing energy consumption and equipment costs. And the required treatment equipment is simple, easy to be compactly integrated and used, and realizes industrial production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a flow chart of recovering barite from the solids discharged from the drilling solids control system of the present invention. SPECIFIC EMBODIMENTS

[0026] To make the objectives, technical solutions and advantages of the embodiments of the present invention clearer, the following will, with reference to the accompanying drawings in the embodiments of the present invention, clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the scope of protection of the present invention.

[0027] Example 1

[0028] A method for recovering barite from solids discharged from a drilling solids control system

[0029] Treatment raw material: The centrifugal slag of polysulfonate drilling fluid discharged from the centrifuge of a drilling solids control system in a certain oilfield, with a density of 2.48 g / cm 3 , and a solid content of 19.8%.

[0030] Treatment steps:

[0031] (1) Add 100 L of centrifugal slag and 200 L of clear water to a mechanical agitation flotation machine in sequence. Under the condition that the agitation speed is 500 revolutions per minute, agitate for 10 minutes to fully disperse the centrifugal slag.

[0032] (2) Prepare a mixed solution of sodium hypochlorite and hydrochloric acid with a concentration of 30% according to the molar ratio of calcium hypochlorite to hydrochloric acid of 1:3, add it to the mechanical agitation flotation machine, and agitate while adding under the condition that the agitation speed is 500 revolutions per minute. Adjust the pH value to 5, and let it stand and settle in a sedimentation tank for about 30 minutes. Transfer the generated floating slag and about 200 L of the upper suspension to a water treatment device.

[0033] (3) Add about 150 L of clear water to the remaining solid precipitate in step (2) to adjust the solid content to 8% v / v. Under the condition that the agitation speed is 500 revolutions per minute, add sodium silicate to adjust the pH value to 10, and let it stand and settle in a sedimentation tank for about 30 minutes. Transfer about 200 L of the upper suspension to a water treatment device.

[0034] (4) Add about 200 L of clear water to the remaining solid precipitate in step (3) to adjust the solid content to 8% v / v. Under the condition of maintaining mechanical agitation, add 1 L of a sodium dodecyl sulfate solution with a concentration of 1% in sequence, and conduct flotation for 5 minutes at a rotation speed of 2000 revolutions per minute. Scrape off the foam floating slag and let it settle to obtain the recovered barite powder.

[0035] (5) Place the recovered barite powder in step (4) in a washing tank, add 50 L of water and a small amount of hydroxyalkyl oil. After mixing, conduct centrifugal dehydration using a horizontal screw centrifuge. The rotation speed of the centrifuge is 1500 revolutions per minute. The centrifugal slag is the recovered barite finished product, and the liquid of the centrifuged suspension is transferred to a water treatment device.

[0036] (6) Adjust the pH value of the solution in the water treatment equipment to 6.5 with 10% sulfuric acid solution and 10% sodium hydroxide solution, perform coagulation treatment with polyaluminum chloride solution and polyacrylamide solution, and centrifuge and separate with a horizontal spiral centrifuge. The centrifuged effluent can be used as makeup water for steps (2) to (5) respectively and can be recycled for formulating drilling fluid. Among them, the dosage of polyaluminum chloride is 100 mg / L; the molecular weight of polyacrylamide is 20 million, and the dosage is 10 mg / L; the rotation speed of the horizontal spiral centrifuge is 2000 revolutions per minute.

[0037] Use the Lee bottle method specified in the "Drilling Fluid Material Specification" of GB / T 5005 - 2010 to measure the recovered barite, and the density reaches 4.14 g / cm 3 .

[0038] Example 2

[0039] A method for recovering barite from solids discharged from a drilling solids control system

[0040] Treatment raw materials: The bottom mud of the circulation tank discharged from a certain oilfield drilling solids control system, with a density of 2.13 g / cm 3 , and the solid content is 21.9%.

[0041] Treatment steps:

[0042] (1) Add 150 L of bottom mud of the circulation tank and 150 L of recycled intermediate water to the first mechanical agitation flotation machine in sequence, and treat for 5 minutes under the condition of 1000 revolutions per minute to fully disperse the solid phase.

[0043] (2) Prepare 5 L of a mixed solution of sodium hypochlorite and sulfuric acid with a concentration of 30% according to the molar ratio of sodium hypochlorite to sulfuric acid of 1:4, add it to the first mechanical agitation flotation machine under the condition of 1000 revolutions per minute, stir and treat for 15 minutes, and then separate through a hydrocyclone. The liquid phase is transferred to the water treatment equipment, and the solid phase is transferred to the second mechanical agitation flotation machine.

[0044] (3) Add about 250 L of recycled intermediate water to the second mechanical agitation flotation machine to adjust the solid content to 10% v / v. Under the rotation speed of 1000 revolutions per minute, add sodium hexametaphosphate solution, fully mix and then separate through a hydrocyclone. The liquid phase is transferred to the water treatment equipment, and the solid phase is transferred to the first mechanical agitation flotation machine.

[0045] (4) Add about 250 L of recycled intermediate water to the first mechanical agitation flotation machine to adjust the solid content to 10% v / v. Under the rotation speed of 2200 revolutions per minute, use 1 L of 1% sodium dodecyl sulfate solution for flotation for 5 minutes, scrape off the foam scum and let it settle to obtain the recovered barite powder.

[0046] (5) Place the barite powder recovered in step (4) into a washing tank, add 50 L of water and a small amount of hydroxyparaffin oil. After mixing, centrifuge and dehydrate using a horizontal scroll centrifuge at a speed of 2000 revolutions per minute. The centrifuged residue is the recovered barite product, and the liquid of the centrifuged suspension is transferred to a water treatment device.

[0047] (6) Adjust the pH value of the solution in the water treatment device to 7 using 10% hydrochloric acid solution and 10% sodium silicate. Conduct coagulation treatment using polyaluminum chloride and polyacrylamide solution, and then perform centrifugal separation. The centrifuged effluent can be used as makeup water for steps (2) to (5) respectively and can be recycled for formulating drilling fluid. Among them, the dosage of polyaluminum chloride is 150 mg / L; the molecular weight of polyacrylamide is 18 million, and the dosage is 20 mg / L; the speed of the horizontal scroll centrifuge is 1800 revolutions per minute.

[0048] Use the Lee bottle method specified in the "Drilling Fluid Material Specification" of "GB / T 5005 - 2010" to measure the recovered barite, and the density reaches 4.16 g / cm 3 .

[0049] Example 3

[0050] A method for recovering barite from solids discharged from a drilling solids control system

[0051] Treatment raw materials: The centrifuged residue of polysulfide drilling fluid discharged from the centrifuge of a certain oilfield drilling solids control system, with a density of 2.63 g / cm 3 , and the solid content is 22.6%.

[0052] Treatment steps:

[0053] (1) Add 150 L of centrifuged residue and 150 L of recycled intermediate water to the first mechanical agitation flotation machine in sequence. Under the condition of a stirring speed of 600 revolutions per minute, stir for 10 minutes to fully disperse the centrifuged residue.

[0054] (2) Prepare 5 L of a mixed solution of hydrogen peroxide and acetic acid with a concentration of 6% according to the molar ratio of hydrogen peroxide:acetic acid of 1:3. Under the condition of a stirring speed of 600 revolutions per minute, stir and treat for 30 minutes, adjust the pH value to 5, and then perform separation treatment using a hydrocyclone. The liquid phase is transferred to a water treatment device, and the solid phase is transferred to the second mechanical agitation flotation machine.

[0055] (3) Add approximately 300 L of recycled intermediate water to the second mechanical agitation flotation machine to adjust the solid content to 6% v / v. At a rotation speed of 600 revolutions per minute, add a sodium hexametaphosphate solution. After fully mixing evenly, perform hydrocyclone separation. The liquid phase is transferred to a water treatment device, and the solid phase is transferred to the first mechanical agitation flotation machine.

[0056] (4) Add about 300 L of recycled intermediate water to the first mechanical agitation flotation machine to adjust the solid content to 6% v / v. At a rotational speed of 2000 revolutions per minute, use 2 L of 1% sodium dodecyl sulfate solution for flotation for 3 minutes. Scrape off the foam scum and let it settle to obtain the recovered barite powder.

[0057] (5) Place the barite powder recovered in step (4) in a washing tank, add 50 L of water and a small amount of hydroxyalkyl oil. After mixing, dehydrate by centrifugation using a horizontal screw centrifuge at a rotational speed of 2500 revolutions per minute. The centrifugal slag is the recovered barite product, and the liquid of the centrifuged suspension is transferred to the water treatment equipment.

[0058] (6) Use 10% sulfuric acid solution and 10% water glass solution to adjust the pH value of the solution in the water treatment equipment to 6.5. Conduct coagulation treatment using polyaluminum ferric chloride and polyacrylamide solution, and then perform centrifugal separation using a horizontal screw centrifuge. The centrifuged effluent can be used as makeup water for steps (2) to (5) respectively and can be recycled for formulating drilling fluid. Among them, the dosage of polyaluminum ferric chloride is 100 mg / L; the molecular weight of polyacrylamide is 20 million, and the dosage is 10 mg / L; the rotational speed of the horizontal screw centrifuge is 2000 revolutions per minute.

[0059] Use the Lee bottle method specified in the "Drilling Fluid Material Specification" of "GB / T 5005 - 2010" to measure the recovered barite, and the density reaches 4.18 g / cm 3 .

[0060] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solutions of the present invention, and these simple modifications all fall within the protection scope of the present invention.

Claims

1. A method for recovering barite from solids discharged from a drilling solids control system, characterized in that, The method includes: Mixing the solids discharged from the drilling solids control system with water to prepare a slurry, obtaining a first slurry; Mixing and stirring the acidic oxidant solution with the first slurry, performing solid-liquid separation, and mixing the obtained solid phase part with water to prepare a slurry, obtaining a second slurry; Mixing and stirring a dispersant with the second slurry, performing solid-liquid separation, and mixing the obtained solid phase part with water to prepare a slurry, obtaining a third slurry; Mixing and stirring a flotation agent with the third slurry and then performing flotation to obtain barite.

2. The method according to claim 1, characterized in that, The solid content in the first slurry is less than 20% v / v.

3. The method according to claim 1, characterized in that, The acidic oxidant solution is a mixed solution of an acid and an oxidant. The oxidant is selected from any one of sodium hypochlorite, calcium hypochlorite, and hydrogen peroxide, and the acid is selected from any one of hydrochloric acid, sulfuric acid, oxalic acid, and acetic acid.

4. The method according to claim 3, characterized in that, In the acidic oxidant solution, the molar ratio of the oxidant to the acid is 1:2 to 5.

5. The method according to claim 1, characterized in that, Adjust the addition amount of the acidic oxidant solution so that the pH value of the mixture liquid of the acidic oxidant solution and the first slurry is 4 to 6.

6. The method according to claim 1, characterized in that, The solid content of the second slurry is 5% to 20% v / v.

7. The method according to claim 1, characterized in that, The dispersant is selected from any one of sodium hydroxide solution, water glass solution, and sodium hexametaphosphate solution.

8. The method according to claim 1, characterized in that, Adjust the addition amount of the dispersant so that the pH of the mixture liquid of the dispersant and the second slurry is 9 to 10.

9. The method according to claim 1, characterized in that, The solid content of the third slurry is 5% to 20% v / v.

10. The method according to claim 1, characterized in that, The method of the solid-liquid separation includes separation using a settling tank or a hydrocyclone separator.

11. The method according to claim 1, characterized in that, The flotation agent is sodium dodecyl sulfate.

12. The method according to claim 11, characterized in that, The addition amount of the flotation agent is 50 to 200 mg / L.

13. The method according to claim 1, characterized in that, It also includes washing the barite obtained by flotation; preferably, washing is performed using a mixed solution of hydroxyl paraffin oil and water.

14. The method according to claim 1, characterized in that, It also includes recovering the water in the waste liquid generated in each step for recycling.

15. The method according to claim 14, characterized in that, The method of recovery is: first adjust the pH value of the waste liquid to 6.5 to 7.0, then perform coagulation treatment using a polyaluminum chloride solution and a polyacrylamide solution, and after completion, perform centrifugal separation to discard the slag, thus obtaining.

Citation Information

Patent Citations

  • A method of recovering barite from waste drilling mud

    CN104609455B