A nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, its preparation method and application

Nano-titanium functional fillers were prepared by using organosilicon-modified epoxy resin and high-energy ball milling to solve the problems of poor corrosion resistance and internal defects of epoxy coatings under high temperature environments, and to achieve long-term protective effects in extreme marine environments.

CN120209705BActive Publication Date: 2026-11-10HARBIN ENG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510502154.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-21
Publication Date
2026-11-10
Estimated Expiration
2045-04-21

AI Technical Summary

Technical Problem

Traditional epoxy coatings have poor corrosion resistance at high temperatures, are prone to internal defects during curing, and have poor dispersibility of nano-functional fillers, making it difficult to effectively protect equipment in extreme marine environments for a long time.

Method used

Nano-titanium functional fillers were prepared by using silicone-modified epoxy resin and high-energy ball milling to form an interpenetrating network structure and a uniformly dispersed coating. Polar and non-polar solvents were used to ensure uniform mixing, and curing conditions were optimized to reduce defects.

Benefits of technology

It improves the coating's high-temperature resistance and corrosion resistance, extends its service life, reduces the production cost of nanofillers, and maintains good protective effects in high-temperature and high-humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120209705B_ABST
    Figure CN120209705B_ABST
Patent Text Reader

Abstract

This invention discloses a nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, its preparation method, and its application. The preparation method includes the following steps: preparing an organosilicon modified epoxy resin and preparing nano-titanium functional fillers; then, taking the prepared organosilicon modified epoxy resin, powder fillers, dispersants, leveling agents, and defoamers, adding them to a mixed solvent, and placing them in a high-speed disperser at 2000-3000 rpm at room temperature to stir, obtaining a mixed slurry; then, adding the nano-titanium functional fillers, and placing them in a high-speed disperser at 2000-3000 rpm at room temperature to stir, obtaining a nano-titanium-organosilicon modified epoxy resin coating; then, adding an amine curing agent to the coating and mixing and stirring, and finally coating it onto the surface of a substrate and drying to obtain a cured coating. This invention prepares a high-temperature resistant coating with excellent comprehensive performance that can provide long-term corrosion protection for high-temperature marine equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of anti-corrosion coating technology, specifically to a nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, its preparation method, and its application. Background Technology

[0002] High-temperature equipment in ships and marine engineering facilities not only faces the challenges of high humidity and high salinity in marine environments, but also the combined effects of prolonged high temperatures, which accelerate corrosion and structural wear, leading to property damage and safety hazards. Applying high-performance, high-temperature resistant, and corrosion-resistant coatings is an effective protective measure to extend the service life of high-temperature marine equipment. These coatings protect the equipment surface from corrosion while exhibiting high-temperature resistance. Developing long-lasting, high-temperature resistant, heavy-duty anti-corrosion coatings for complex and harsh marine environments and long-term high-temperature corrosion is a pressing problem that needs to be solved.

[0003] Epoxy-based coatings are among the most widely used coatings in marine corrosion protection. The epoxy resin molecule contains polar functional groups such as hydroxyl and ether bonds, resulting in excellent substrate adhesion. Simultaneously, the benzene rings in the molecular chain provide the coating with good rigidity, hardness, and chemical stability. Epoxy resin coatings, prepared by modification and combination with various functional fillers and additives, can be used for corrosion protection in various applications, and are characterized by scalability and ease of application. However, epoxy resin-based coatings still present the following challenges when preparing high-temperature, heavy-duty anti-corrosion coatings:

[0004] Question 1: Epoxy coatings have poor high-temperature resistance.

[0005] Compared to silicone resin coatings, which have excellent high-temperature resistance, epoxy resin coatings have good mechanical properties and substrate adhesion after curing. However, cured epoxy resin will undergo high-temperature oxidation at temperatures above 180°C in air, resulting in poor high-temperature resistance. When equipment is exposed to high-temperature corrosive environments for a long time, traditional epoxy coatings are more prone to failure, and their service life cannot meet industrial requirements.

[0006] Question 2: Various defects can occur inside the epoxy coating during the curing process.

[0007] Epoxy coatings are formed by the rapid cross-linking reaction between epoxy resin and a curing agent. The internal stress generated by this rapid cross-linking reaction cannot be effectively released, leading to micro-cracks within the coating. Simultaneously, the coating also develops pores due to the significant evaporation of solvents. Therefore, various corrosive media can penetrate into the substrate through these pores, and high temperatures further accelerate the breakage of the resin molecular chains, ultimately causing the coating to fail and unable to provide long-term protection to the metal substrate.

[0008] Question 3: Nanofunctional fillers have high preparation costs and poor dispersibility in coatings.

[0009] Nanomaterials possess a large specific surface area and small size, generally exhibiting superior physicochemical properties compared to traditional materials. As functional fillers, they can not only improve the conventional properties of coatings but also impart other special functions. However, the application of nanofillers in the field of anti-corrosion coatings still faces challenges. First, compared to traditional functional fillers, the preparation of nanofunctional fillers is limited by technological processes, resulting in small-scale production and higher costs. Second, nanomaterials have high surface energy and exhibit interaction forces, making nanoparticles or sheets prone to agglomeration. This leads to poor dispersibility in silicone-modified epoxy resins, causing various defects within the coating during curing and reducing the service life of the anti-corrosion coating. Therefore, reducing the production cost of nanofunctional fillers, expanding production scale, and solving the dispersibility problem in coatings are pressing challenges that need to be addressed in the research of anti-corrosion coatings.

[0010] Question 4: Traditional epoxy coatings are difficult to simultaneously cope with high temperatures and extreme marine composite corrosion environments.

[0011] Epoxy coatings can improve high-temperature stability and meet corrosion resistance requirements in ordinary atmospheric environments by adding high-temperature resistant fillers such as aluminum powder, phosphates, and chromium oxide. However, for marine engineering equipment operating in extreme marine environments and requiring high-temperature operation, the aforementioned epoxy-based composite coatings clearly cannot meet long-term protection requirements. Therefore, developing high-temperature resistant anti-corrosion coatings suitable for extreme marine environments remains a pressing challenge. Summary of the Invention

[0012] In view of this, and in view of the problems existing in the prior art, the purpose of this invention is to provide a nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, its preparation method and application, which effectively solves the problems of poor corrosion resistance and high temperature resistance after curing of traditional epoxy anti-corrosion coatings, various internal defects generated during rapid curing, and poor dispersion of functional fillers in the coating.

[0013] The technical solution adopted is as follows:

[0014] The present invention discloses a method for preparing a nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, comprising the following steps:

[0015] S1. Mix epoxy resin and xylene solvent evenly, add silicone resin and remove water under vacuum; add silane coupling agent and dibutyltin dilaurate, heat to 80-100℃ and stir at a constant speed to obtain silicone modified epoxy resin.

[0016] S2. Titanium powder, silicone resin and grinding aid are put into a high-energy ball mill. The titanium powder, silicone resin and grinding aid are ground at high speed at room temperature and a rotation speed of 1000-3000 rpm to obtain a black paste-like substance, which is the nano-titanium functional filler.

[0017] S3. First, take the silicone-modified epoxy resin, powder filler, dispersant, leveling agent, and defoamer prepared in S1, add them to the mixed solvent, and place them in a high-speed disperser at 2000-3000 rpm at room temperature to stir and obtain a mixed slurry; then, add nano-titanium functional filler, place it in a high-speed disperser at 2000-3000 rpm at room temperature to stir and obtain a nano-titanium-silicone-modified epoxy resin coating;

[0018] S4. Add an amine curing agent to the coating and mix thoroughly. Finally, apply the mixture to the substrate surface and dry to obtain a cured coating.

[0019] Furthermore, in S1, the epoxy resin is one or more of E20, E44, E51, and F44; and / or, in S1 and S2, the silicone resin is one or more of polymethyl silicone resin, polyaryl silicone resin, and methylphenyl silicone resin.

[0020] Further, in S1, the mass ratio of the silicone resin to the epoxy resin is (1-2):1; and / or, in S2, the mass ratio of the titanium powder to the silicone resin is 5:(2-6).

[0021] Further, in S2, the grinding aid is one or more of xylene, dichloromethane, and acetone; and / or, the titanium powder is high-purity industrial titanium powder with a purity ≥ 99.95%.

[0022] Further, in S2, the grinding aid is one or more of xylene, dichloromethane, and acetone; and / or, the titanium powder is high-purity industrial titanium powder with a purity ≥ 99.95%.

[0023] Furthermore, in S2, high-speed grinding is performed for 2-8 hours at room temperature and a rotation speed of 1000-3000 rpm.

[0024] Furthermore, in S3, the powder filler is one or more of talc, fumed silica, titanium dioxide, and nano-alumina; and / or, the mixed solvent is a mixture of polar and non-polar solvents.

[0025] Further, in S5, the coating is applied to the surface of the substrate and placed in a forced-air drying oven at 100-150℃ for 5-12 hours to obtain a cured coating.

[0026] Furthermore, in S5, the thickness of the cured coating is 100±10μm.

[0027] Furthermore, in S5, the substrate is Q235 carbon steel with surface pretreatment.

[0028] The present invention provides a nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, which is prepared by the preparation method described in any of the above schemes.

[0029] The application of the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating described above in the present invention for surface protection of equipment on marine oil and gas platforms.

[0030] In the above technical solution:

[0031] 1. When synthesizing silicone-modified epoxy resin, the epoxy resin needs to be dehydrated under vacuum to ensure that a stable silicone-modified epoxy resin is obtained.

[0032] 2. Synthesize nano-titanium functional fillers. The high-energy ball mill has a rotation speed of 1000-3000 rpm and a preferred grinding time of 2-8 hours. This ensures that the grinding balls can fully contact and compress with the titanium powder, organosilicon, and grinding aid. The mechanical energy generated breaks down and pulverizes the titanium particles, making their particle size nano-sized, and allows the organosilicon resin to fully coat the surface of the nano-titanium particles.

[0033] 3. When preparing the coating, use a mixture of polar and non-polar solvents to ensure uniform mixing of the silicone-modified epoxy resin and the functional filler. Polar solvents may include, for example, one or more of N,N-dimethylformamide (DMF), n-butanol, cyclohexanone, and dichloromethane; non-polar solvents may include, for example, one or more of toluene and xylene.

[0034] 4. The preferred curing conditions for the coating are to place it in a 100-150℃ forced-air drying oven for 5-12 hours. The resin cross-linking and curing reaction rate is moderate with the solvent evaporation rate inside the coating. The coating has sufficient time to level during curing, reducing internal defects after complete curing.

[0035] Features of this invention:

[0036] Feature 1: The silicone-modified epoxy resin used as the coating solves the problem of poor high-temperature resistance of traditional epoxy resin coatings. Silicone resins, with Si-O-Si bonds as the main molecular chain segments, have high bond energies and form a Si-O-based cross-linked network structure after curing, exhibiting excellent high-temperature resistance and weather resistance. Modifying epoxy resin with silicone resin can effectively improve the resin's high-temperature resistance. This invention utilizes a simple and easy-to-operate synthesis process to mechanically blend silicone and epoxy resin molecular chain segments to form an interpenetrating network structure, preparing a stable silicone-epoxy resin system as a composite coating, thereby improving the high-temperature resistance of the base epoxy resin.

[0037] Feature 2: The nano-titanium functional filler prepared by high-energy ball milling exhibits excellent dispersibility in silicone-modified epoxy resin. Raw titanium powder, silicone resin, and grinding aid are fed into a high-energy ball mill. The balls collide with the raw materials as they roll, causing the titanium powder to break down due to impact, reducing the particle size to the nanoscale and significantly increasing its surface energy. Simultaneously, the high energy generated by the collisions between the balls allows the silicone resin to coat the metal particles, thus obtaining the nano-titanium functional filler. When this filler is thoroughly mixed with silicone-modified epoxy resin, the silicone resin coating of the titanium particles effectively reduces the surface energy and interactions of the nanoparticles, hindering agglomeration and improving dispersibility in the silicone-modified epoxy resin. This solves the problem of poor dispersibility of nano-functional fillers in silicone-modified epoxy resin and slows down sedimentation, ensuring the quality of the coating during long-term storage.

[0038] Feature 3: The addition of nano-titanium functional fillers can effectively reduce internal defects generated during coating curing and improve the long-term corrosion resistance, alternating stress resistance, and service life of the coating. When nano-titanium functional fillers are uniformly dispersed in the coating, fewer micropores and cracks are generated during the rapid curing process, thereby reducing the channels for corrosive media to penetrate and diffuse into the coating. Due to the stable chemical properties and strong corrosion resistance of titanium, it can effectively block corrosive media. At the same time, nano-titanium has higher thermal conductivity than silicone-modified epoxy resin. In high-temperature environments, the uniform dispersion of nano-titanium in the coating can effectively conduct heat, reducing coating defects caused by heat concentration, so that the composite coating can maintain its anti-corrosion performance in long-term high-temperature environments.

[0039] Therefore, the beneficial effects of the present invention are as follows:

[0040] 1. This invention synthesizes an organosilicon-modified epoxy resin with good high-temperature resistance as a coating material, which can effectively cope with the harsh and complex marine environment and the combined corrosion factors of high temperature, and improve the service life of the coating.

[0041] 2. This invention utilizes high-energy ball milling to prepare nano-titanium with excellent dispersibility in the organosilicon-modified epoxy resin as a functional filler, which provides effective barrier protection for the coating while reducing internal defects in the coating.

[0042] 3. This invention utilizes the excellent high-temperature resistance of silicone-modified epoxy resin and the synergistic protective effect of nano-titanium functional filler's good dispersion, barrier, and thermal conductivity to prepare a high-temperature resistant coating with excellent comprehensive performance that can provide long-term corrosion protection for high-temperature marine equipment.

[0043] 4. The nano-titanium functional filler prepared by the high-energy ball milling method of this invention has low cost and great industrialization potential. This nano-titanium functional filler has good compatibility with organosilicon-modified epoxy resin. The resulting nano-composite modified epoxy coating, after curing, has fewer internal defects and is more dense than traditional composite modified epoxy coatings. It exhibits strong corrosion resistance, and due to the uniform distribution of the nano-titanium functional filler within the coating, the coating possesses excellent thermal conductivity, thereby improving the coating's high-temperature resistance. Attached Figure Description

[0044] Figure 1 Infrared spectra of methylphenyl silicone resin (SL), nano-titanium functional filler (STiN), and raw material titanium powder (Ti).

[0045] Figure 2 Transmission electron microscopy image of nano-titanium functional filler (STiN).

[0046] Figure 3 The graph shows the water absorption rate of the coating after 240 hours.

[0047] Figure 4 The electrochemical impedance spectroscopy spectrum is shown after the coating has been immersed for 360 hours.

[0048] Figure 5 The coating resistance R is fitted to the electrochemical AC impedance test data after the coating is immersed for 360 hours. c Bar chart.

[0049] Figure 6 A bar chart showing the low-frequency impedance modulus of the coating after high-temperature, high-humidity, and high-salt cycling experiments, based on electrochemical impedance spectroscopy.

[0050] Figure 7 Optical photographs of the surface morphology of the coating after a high-temperature, high-humidity, and high-salt cycling experiment. Detailed Implementation

[0051] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0052] Example 1

[0053] The preparation method of the nano-titanium-organic silicon modified epoxy resin anti-corrosion coating in this embodiment includes the following steps:

[0054] Step 1: Mix 200g of epoxy resin and 20g of xylene solvent evenly, add 200g of methylphenyl silicone resin and vacuum dehydrate for 1 hour. Add 12g of silane coupling agent KH550 and 3g of dibutyltin dilaurate, heat to 90℃ and stir at a constant speed for 2 hours to obtain silicone-modified epoxy resin, with a solid content of approximately 95.4%.

[0055] Step 2: Synthesis of nano-titanium filler: 500g of high-purity industrial titanium powder (purity ≥99.95%), 500g of methylphenyl silicone resin and grinding aid were put into a high-energy ball mill. The titanium powder, silicone and grinding aid xylene were ground at high speed for 4 hours at room temperature and a rotation speed of 1600 rpm to obtain a black paste-like substance, which is the nano-titanium functional filler (STiN).

[0056] Step 3: First, take 130g of silicone-modified epoxy resin, 11g of talc powder, 1.8g of R972 powder, 0.5% of dispersant, leveling agent, and defoamer by mass of silicone-modified epoxy resin, add them to a mixed solvent of 30g xylene and 10g n-butanol, and place them in a high-speed disperser and stir at 3000rpm at room temperature for 1h to obtain a composite slurry.

[0057] Step 4: Add 20% (by mass) of T31 type phenolic amine curing agent to the coating and mix thoroughly. Apply the cured system to the surface of a pretreated Q235 carbon steel sheet with dimensions of 60mm × 30mm × 3mm, and place it in a 100℃ forced-air drying oven for 6 hours to obtain a cured coating. The thickness of the cured coating is 100±10μm.

[0058] Figure 1 Infrared spectra of methylphenyl silicone resin (SL), prepared titanium nanoparticles (STiN), and raw titanium powder (Ti). The characteristic peak at 1064 cm⁻¹ in the SL infrared spectrum corresponds to the Si-O-Si stretching vibration absorption peak of silicone. The same group appears in the infrared spectrum of STiN, and a peak at 650 cm⁻¹ is also observed. -1 and 472cm -1 The presence of titanium oxide indicates that the high-energy ball milling technology successfully coated the grinding aid SL onto the surface of the titanium particles.

[0059] Figure 2 Transmission electron microscopy (TEM) image of the prepared STiN. It can be seen that the raw material Ti was pulverized to nanoscale particle size using high-energy ball milling, and the morphology of the nano-titanium functional filler is that of relatively thin nanosheets.

[0060] Example 2

[0061] This embodiment is basically the same as embodiment 1, except that in step 1, 300g of methylphenyl silicone resin is added and vacuum dehydrated for 1 hour.

[0062] Example 3

[0063] This embodiment is basically the same as embodiment 2, except that in step 3, 10% of nano-titanium functional filler with organosilicon modified epoxy resin is added and stirred in a high-speed disperser at 2400 rpm for 4 hours at room temperature to obtain nano-titanium-organosilicon modified epoxy coating.

[0064] Example 4

[0065] This embodiment is basically the same as embodiment 3, except that in step 3, an additional 12% nano-titanium functional filler of organosilicon modified epoxy resin is added and stirred in a high-speed disperser at 2400 rpm for 4 hours at room temperature to obtain nano-titanium-organosilicon modified epoxy coating.

[0066] Example 5

[0067] This embodiment is basically the same as embodiment 3, except that in step 3, 15% of nano-titanium functional filler with organosilicon modified epoxy resin is added and stirred in a high-speed disperser at 2400 rpm at room temperature for 4 hours to obtain nano-titanium-organosilicon modified epoxy coating.

[0068] Comparative Example 1

[0069] E44 epoxy resin was mixed with T31 ​​curing agent and stirred evenly. The cured system was then applied to the surface of Q235 carbon steel with dimensions of 60mm×30mm×3mm after surface sandblasting. The cured coating was then placed in an 80℃ forced-air drying oven for 4 hours to obtain a cured coating with a thickness of 100±10μm.

[0070] Test Result Analysis

[0071] 1. Pull-out adhesion test

[0072] The standard reference for the coating pull-out adhesion test in all embodiments is GB / T 5210-2006. The testing instrument is the PosiTest ATA-B pull-out adhesion tester. The test results are shown in Table 1.

[0073] In Examples 1 and 2, the silicone-modified epoxy resin coating exhibits good substrate adhesion.

[0074] The test results of Examples 3, 4 and 5 show that adding an appropriate amount of nano-titanium polymer functional filler will not affect the adhesion of the silicone-modified epoxy resin coating.

[0075] Table 1. Results of Coating Pull-out Adhesion Test

[0076]

[0077] 2. Coating water absorption rate test

[0078] The experimental standard for testing the water absorption rate of the coatings in all examples and comparative examples is HG / T 3344-2012. After the dry weight of the cured sample coating is tested, it is immersed in a 3.5wt% sodium chloride solution. After that, it is taken out at specific time intervals, the surface water is wiped off, and the weight is weighed to calculate the water absorption rate. The test duration is 240h.

[0079] The test results are attached. Figure 3 As shown, all coatings reached water saturation after 24 hours. Comparative Example 1 (epoxy resin cured coating) had the highest saturation water absorption rate. The test results of Example 1 and Example 2 show that the saturation water absorption rate of the silicone-modified epoxy resin coating decreased. This is because the introduction of methylphenyl silicone resin modification led to a reduction in epoxy resin curing defects and an improvement in the coating's water repellency.

[0080] The test results of Examples 3, 4 and 5 show that introducing an appropriate amount of nano-titanium polymer functional filler can further reduce the water absorption rate of the coating. This is because the functional filler has good dispersion compatibility in organosilicon modified epoxy resin, improves the density of the cured coating, and plays a role in blocking the diffusion of water molecules in the cured coating.

[0081] 3. Electrochemical testing

[0082] The corrosion resistance of the coatings in all examples and comparative examples was tested using electrochemical impedance spectroscopy. The testing platform was a Metrohm PGSTST302N electrochemical workstation. A three-electrode system was selected, with the coated carbon steel sheet as the working electrode (test area radius 1 cm), a saturated calomel electrode as the reference electrode, a platinum sheet electrode as the counter electrode, and a 3.5 wt% sodium chloride solution as the electrolyte. The test frequency range was 10 Hz. 5 -10 -2 The Hz, sinusoidal signal amplitude of 10mV, all examples and comparative examples of coatings were immersed in 3.5wt% sodium chloride solution for 360h and then subjected to electrochemical impedance testing. The test results were fitted using ZView2 software.

[0083] The Bode plot of the electrochemical impedance spectroscopy is attached. Figure 4 As shown in the Bode plot, the low-frequency impedance modulus |Z| 0.01Hz The size directly reflects the corrosion resistance of the coating. After immersion in a 3.5wt% sodium chloride solution for 360 hours, the low-frequency impedance modulus |Z| of the coating in Comparative Example 1 was [not specified]. 0.01Hz At the very least, the test results of Examples 1 and 2 show that the long-term corrosion resistance of the silicone-modified epoxy resin coating is significantly improved compared to the epoxy coating. This is because the introduction of silicone prepolymer molecular chain segments reduces curing defects in the epoxy resin, improves water repellency, and enhances the barrier properties against corrosive media.

[0084] The test results from Examples 3, 4, and 5 show that introducing an appropriate amount of nano-titanium polymer functional filler can further enhance the corrosion resistance of the coating. This is because the functional filler has good dispersion compatibility in the silicone-modified epoxy resin, which improves the density of the cured coating. The chemically stable titanium nanoparticles can effectively block the diffusion of corrosive media to the coating-metal substrate interface, thus improving the long-term corrosion resistance of the coating.

[0085] Electrochemical impedance data were fitted to obtain the coating resistance values ​​R of the examples and comparative examples. c As attached Figure 5 As shown. The coating resistance R in Example 3 is... c It has the highest corrosion resistance.

[0086] 4. High temperature, high humidity, and high salt corrosion resistance test

[0087] The high-temperature and corrosion resistance of the coatings in all embodiments were assessed using a high-temperature, high-humidity, and high-salt cyclic test. For the high-temperature test, the coating samples were calcined in air at 300°C for 24 hours in a muffle furnace. For the high-humidity and high-salt test, a neutral salt spray test was conducted, referencing GB / T 31588.1-2015. The temperature was set to 35°C, and the salt spray solution was a 5% wt% sodium chloride solution. After calcination, the coating samples were placed in a salt spray chamber for 24 hours. The samples were then removed and subjected to electrochemical impedance spectroscopy (EIS) testing to analyze their barrier properties. This cycle was repeated until the coating completely failed. The electrochemical test results are attached. Figure 6 As shown.

[0088] The coatings in Examples 1 and 2 completely failed after five high-temperature, high-humidity, and high-salt cycling experiments. The coating morphology is shown in the attached figure. Figure 7 As shown, the coating surface is exposed to high temperatures for a long time, and the resin molecules undergo thermal decomposition, resulting in a large number of cracks. The obvious corrosion sites indicate that there are defects inside the coating at the same time. Neutral salt spray can quickly diffuse from the coating to the metal substrate interface, causing corrosion.

[0089] Examples 3, 4, and 5 maintained certain barrier properties after six high-temperature, high-humidity, and high-salt cycling tests, indicating that the introduction of an appropriate amount of nano-titanium polymer functional filler enhances the high-temperature corrosion resistance of the coating. This is because the functional filler has good dispersion compatibility in the silicone-modified epoxy resin, improving the crosslinking degree of the cured resin. The uniformly dispersed nano-titanium particles also increase the thermal conductivity of the cured coating, to some extent avoiding coating structural damage caused by heat concentration, while simultaneously blocking the diffusion of corrosive media. The coating morphology of Examples 3, 4, and 5 after six cycles is shown in the attached figure. Figure 7As shown, the coating surface has cracks but no corrosion sites. Among them, the coating of Example 3 has the highest impedance modulus and fewer surface cracks, exhibiting relatively excellent high-temperature corrosion resistance.

[0090] The above are merely preferred embodiments of the present invention and do not constitute any limitation on the present invention. Although the present invention has been described through the above embodiments, any adjustments, equivalent modifications, and simple improvements made by those skilled in the art without departing from the spirit, principles, and technical requirements of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a nano-titanium-organosilicon modified epoxy resin anti-corrosion coating, characterized in that, Includes the following steps: S1. Mix epoxy resin and xylene solvent evenly, add silicone resin and remove water under vacuum; add silane coupling agent and dibutyltin dilaurate, heat to 80-100℃ and stir at a constant speed to obtain silicone modified epoxy resin. S2. Titanium powder, silicone resin and grinding aid are put into a high-energy ball mill. The titanium powder, silicone resin and grinding aid are ground at high speed at room temperature and a rotation speed of 1000-3000 rpm to obtain a black paste-like substance, which is the nano-titanium functional filler. S3. First, take the silicone-modified epoxy resin, powder filler, dispersant, leveling agent, and defoamer prepared in S1, add them to the mixed solvent, and place them in a high-speed disperser at 2000-3000 rpm at room temperature to stir and obtain a mixed slurry; then, add nano-titanium functional filler, place it in a high-speed disperser at 2000-3000 rpm at room temperature to stir and obtain a nano-titanium-silicone-modified epoxy resin coating; S4. Add an amine curing agent to the coating and mix thoroughly. Finally, apply the mixture to the substrate surface and dry to obtain a cured coating.

2. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S1, the epoxy resin is one or more of E20, E44, E51, and F44; and / or, in S1 and S2, the silicone resin is one or more of polymethyl silicone resin, polyaryl silicone resin, and methylphenyl silicone resin.

3. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S1, the mass ratio of the silicone resin to the epoxy resin is (1-2):1; and / or, in S2, the mass ratio of the titanium powder to the silicone resin is 5:(2-6).

4. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S1, the silane coupling agent is one or more of KH550, KH560, KH570, and KH590.

5. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S2, the grinding aid is one or more of xylene, dichloromethane, and acetone; and / or, the titanium powder is high-purity industrial titanium powder with a purity ≥ 99.95%.

6. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S3, the powder filler is one or more of talc, fumed silica, titanium dioxide, and nano alumina; and / or, the mixed solvent is a mixture of polar and non-polar solvents.

7. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S4, the coating is applied to the surface of the substrate and placed in a 100-150℃ forced-air drying oven for 5-12 hours to obtain a cured coating.

8. The method for preparing the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating according to claim 1, characterized in that, In S4, the thickness of the cured coating is 100±10μm.

9. A nano-titanium-organic silicon modified epoxy resin anti-corrosion coating, characterized in that, It is prepared by the preparation method described in any one of claims 1-8.

10. The application of the nano-titanium-organosilicon modified epoxy resin anti-corrosion coating of claim 9 in the surface protection of equipment on marine oil and gas platforms.

Citation Information

Patent Citations

  • Long-acting anticorrosive weatherproof functional coating and preparation method thereof

    CN108841289A

  • Fireproof heat insulation coating and preparation method thereof

    CN110105800A