Analysis method for accurately positioning plaque defect substrate on surface of coated plate
Through the focusing ion beam method, multi-point positioning and cutting and micromorphic analysis of the coated plate samples was solved, and the problem of difficult to accurately analyze the corresponding relationship between spot-like defects on the surface of the coating and the substrate was achieved, and the accurate exploration of the causes of the defect was achieved.
Patent Information
- Application Number
- CN202510430281.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-08
- Publication Date
- 2025-06-27
AI Technical Summary
The prior art is difficult to accurately analyze the correspondence between spotted defects on the surface of the coating and the substrate, making it difficult to find out the causes of the defects.
The focused ion beam method was used to perform multi-point positioning and cutting of the coated plate samples to form a multi-point connection area, and the images of the plating and substrate were obtained through micromorphic analysis, and the causes of the defect were determined by comparative analysis.
The accuracy of the analysis position of the spotted defect on the surface of the coating and the corresponding relationship between the substrate is improved, and the causes of the defect can be accurately explored.
Smart Images

Figure CN120214000A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of analysis of surface quality defects of coated plates, and particularly to an analysis method for accurately positioning the substrate of patchy defects on the surface of coated plates. Background Art
[0002] In order to prevent corrosion on the surface of steel plates and extend their service life, it is often necessary to coat a layer of metallic zinc on their surface. This method is currently the most common and effective anti-corrosion measure, and this galvanized thin steel plate is called a galvanized plate. In order to further improve the corrosion resistance and welding performance of steel plates, alloying treatment is often carried out after hot-dip galvanizing to allow the iron in the steel substrate to diffuse with zinc to form a zinc-iron alloy phase coating.
[0003] However, after alloying, patchy defects are likely to appear on its surface. There is a relatively clear corresponding relationship between the formation of such surface quality defects and the surface state or defects of its substrate. The conventional analysis method is to first use a cutter to mark the designated positions of the patchy defects on the surface of the coating, then use a scanning electron microscope to observe and analyze the defects at the designated positions, and then use hydrochloric acid solution to remove the coating to observe the microscopic morphology of the substrate at the marked positions. However, the correspondence between the analysis positions of the patchy defects on the surface of the coating and the substrate is not accurate enough, resulting in the difficulty of accurately reflecting the correspondence between the surface state of the substrate and the patchy defects on its coating surface, and thus it is difficult to find out the reasons for the formation of patchy defects. Summary of the Invention
[0004] This application provides an analysis method for accurately positioning the substrate of patchy defects on the surface of coated plates to solve the following technical problem: how to improve the accuracy of the correspondence between the analysis positions of patchy defects on the coating surface and the substrate.
[0005] In a first aspect, an embodiment of this application provides an analysis method for accurately positioning the substrate of patchy defects on the surface of coated plates, and the method includes:
[0006] Pre-treat the coated plate sample;
[0007] Use the focused ion beam method to perform multi-point positioning cutting on the patchy defect positions of the pre-treated coated plate sample. The number of cutting points for the multi-point positioning cutting is not less than 3, and the cutting depth of each cutting point is greater than the coating thickness of the coated plate sample;
[0008] Connect each of the cutting points to form a multi-point connection area to obtain the coated plate sample to be analyzed;
[0009] Perform microscopic morphology analysis on the multi-point connection area of the coated plate sample to be analyzed to obtain a first image;
[0010] Remove the surface coating of the coated plate sample to be analyzed to obtain a substrate sample;
[0011] Perform microscopic morphology analysis on the multi-point connection area corresponding to the substrate sample to obtain a second image;
[0012] Analyze the reasons for the patchy defects on the coating surface of the coated plate sample based on the first image and the second image.
[0013] Optionally, the size requirements for the cutting points are as follows: the length is 15 μm to 30 μm, and the width is 10 μm to 15 μm.
[0014] Optionally, the beam current of the focused ion beam method is 15 nA to 30 nA.
[0015] Optionally, the stripping solution used for stripping is a mixed solution of concentrated hydrochloric acid and water.
[0016] Optionally, the volume ratio of the concentrated hydrochloric acid to the water is (5 - 10):(5 - 10).
[0017] Optionally, the coated plate sample includes one of the following: galvanized sheet, alloyed galvanized sheet, aluminum-zinc sheet, zinc-aluminum-magnesium sheet.
[0018] Optionally, the size requirements for the coated plate sample are as follows: the length is 5 mm to 10 mm, the width is 5 mm to 10 mm, and the thickness is 0.5 mm to 3 mm.
[0019] Optionally, the patchy defects include at least one of the following: black dot defect, bright dot defect, strip defect, linear defect.
[0020] Optionally, the pretreatment of the coated plate sample includes:
[0021] Mark the positions of the patchy defects on the coated plate sample;
[0022] Clean the marked coated plate sample.
[0023] Optionally, the marking method includes one of the following: drawing an arrow, drawing a line, drawing a circle; and / or,
[0024] The cleaning solution used for cleaning includes at least one of the following: alcohol, acetone.
[0025] The above technical solutions provided by the embodiments of the present application have the following advantages compared with the prior art:
[0026] The analysis method for accurately positioning the substrate of the patchy defects on the surface of the coated plate provided by the embodiment of the present application includes: preprocessing the coated plate sample; using the focused ion beam method to perform multi-point positioning cutting on the patchy defect positions of the preprocessed coated plate sample, the number of cutting points for the multi-point positioning cutting is not less than 3, and the cutting depth of each cutting point is greater than the coating thickness of the coated plate sample; connecting each of the cutting points to form a multi-point connection area to obtain the coated plate sample to be analyzed; performing microscopic morphology analysis on the multi-point connection area of the coated plate sample to be analyzed to obtain a first image; removing the surface coating of the coated plate sample to be analyzed to obtain a substrate sample; performing microscopic morphology analysis on the corresponding multi-point connection area of the substrate sample to obtain a second image; analyzing the causes of the patchy defects on the coating surface of the coated plate sample according to the first image and the second image. This method improves the accuracy of the corresponding relationship between the analysis position of the patchy defects on the coating surface and the substrate. The multi-point positioning cutting is carried out on the preprocessed coated plate using the focused ion beam method, and the number of cutting points is not less than 3. Compared with single-point cutting, multi-point positioning cutting can more accurately locate the defect area and is more likely to quickly and accurately find the position of the patchy defects in the subsequent electron beam mode; the cutting depth of each cutting point is greater than the coating thickness, which can ensure that the coating is penetrated and reach the substrate directly, so that the information obtained in the subsequent analysis of both the coating surface and the corresponding position of the substrate is coherent and complete, and the defect causes can be accurately explored; the first image is obtained by performing microscopic morphology analysis on the multi-point connection area, and the microscopic structure inside the coating can be clearly seen, and it can be explored whether the defect originates from the coating; after the surface coating of the coated plate is removed, the second image is obtained by performing microscopic morphology analysis on the corresponding multi-point connection area of the substrate sample. By comparing the first image and the second image, it can be checked whether the defect occurs at the bonding interface between the coating and the substrate or there are originally defects in the substrate itself, because the two images respectively reflect the microscopic conditions of the same position of the coating and the substrate; according to the comparison results of the first image and the second image, the causes of the patchy defects on the coating surface of the coated plate sample are deeply analyzed. This all-round analysis method from the coating to the substrate, from the cross-section to the surface greatly improves the accuracy of the corresponding relationship between the position of the patchy defects on the coating surface and the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings herein are incorporated into the specification and constitute a part of this specification, showing embodiments consistent with the present application and used together with the specification to explain the principles of the present application.
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the following will briefly introduce the drawings required for the description of the embodiments or the prior art. Obviously, for those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative efforts.
[0029] Figure 1 It is a schematic flow chart of an analysis method for accurately positioning a substrate with patchy defects on the surface of a coated plate provided by an embodiment of the present application;
[0030] Figure 2 It is a topographic map of patchy defects with marks of an alloyed galvanized steel sheet sample provided by Embodiment 1 of the present application;
[0031] Figure 3 It is a triangular positioning cutting topographic map of patchy defects of an alloyed galvanized steel sheet sample provided by Embodiment 1 of the present application;
[0032] Figure 4 It is a surface topographic map of a substrate sample after removing the zinc layer of an alloyed galvanized steel sheet sample provided by Embodiment 1 of the present application. Detailed implementation manners
[0033] To make the objectives, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present application. Obviously, the described embodiments are some but not all of the embodiments of the present application. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present application without creative efforts shall fall within the scope of protection of the present application.
[0034] The various embodiments of the present application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be construed as a rigid limitation on the scope of the present application; therefore, it should be considered that the described range description has specifically disclosed all possible sub-ranges and individual values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and individual numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any cited number (fraction or integer) within the indicated range.
[0035] In this application, unless otherwise stated, the orientation terms such as "upper" and "lower" specifically refer to the drawing direction in the attached drawings. Additionally, in the description of this application's specification, terms such as "including" and "comprising" mean "including but not limited to". In this text, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this text, "and / or" describes the association relationship of associated objects, indicating that three relationships can exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. Where A and B can be singular or plural. In this text, "at least one" means one or more, and "multiple" means two or more. "At least one kind", "at least one item (one) below" or similar expressions refer to any combination of these items, including any combination of single item (one) or plural items (ones). For example, "at least one item (one) of a, b, or c", or, "at least one item (one) of a, b, and c" can both represent: a, b, c, a - b (that is, a and b), a - c, b - c, or a - b - c, where a, b, and c can be single or multiple respectively. In the proportional relationships involved in this text, the parameters that need to be described by proportion should be understood as the antecedents of the proportional formula in the order of description, and the proportional numbers should be understood as the consequents of the proportional formula. For example, if the mass ratio of substance A, substance B, and substance C is 1:2:3, then substance A, substance B, and substance C should correspond one by one with the proportional numbers in the proportional formula in the order of description, that is, the mass of substance A: the mass of substance B: the mass of substance C = 1:2:3.
[0036] Unless otherwise specifically stated, all kinds of raw materials, reagents, instruments, equipment, etc. used in this application can be obtained through market purchase or can be prepared by existing methods.
[0037] In a first aspect, an analysis method for accurately positioning a substrate with patchy defects on the surface of a coated plate is provided in an embodiment of this application. Figure 1 It is a schematic flow chart of an analysis method for accurately positioning a substrate with patchy defects on the surface of a coated plate provided in an embodiment of this application; please refer to Figure 1 The method includes:
[0038] S1. Pretreat the coated plate sample.
[0039] In some embodiments, the pretreatment of the coated plate sample includes:
[0040] Mark the position of the patchy defect on the coated plate sample.
[0041] Clean the marked coated plate sample.
[0042] In some embodiments, the marking methods include one of the following: drawing arrows, drawing lines, and drawing circles; and / or, the cleaning liquid used for cleaning includes at least one of the following: alcohol, acetone.
[0043] In the embodiments of the present application, the position of the patchy defect on the coated plate sample is first marked. A scalpel is used to make a macroscopic mark on the position of the patchy defect. The marking methods include optional methods such as drawing arrows, drawing lines, and drawing circles, that is, drawing arrows, drawing lines, or drawing circles around the patchy defect to roughly mark the approximate position. These simple and intuitive marking means can enable the operator to quickly locate the target defect position. Especially in subsequent cleaning and other complex operation processes, it will not be lost in the key observation area of the sample, providing a clear guide for precise cutting and analysis. Common organic solvents such as alcohol and acetone are used as the cleaning liquid to clean the marked sample. Both alcohol and acetone have good solubility, can effectively remove impurities such as oil stains and dust on the surface of the coated plate, reduce the interference of impurities on focused ion beam cutting and microscopic morphology analysis, and ensure the accuracy and reliability of the analysis results.
[0044] In some embodiments, the patchy defect includes at least one of the following: black dot defect, bright dot defect, strip defect, linear defect.
[0045] In the embodiments of the present application, the patchy defect refers to a regular or irregular shaped dot defect at the nanometer scale visible to the naked eye. The patchy defect covers various forms such as black dot defects, bright dot defects, strip defects, and linear defects. The causes behind different types of defects are often different. The black dot defect may be related to residual impurity particles in the coating, the bright dot defect may involve abnormal reflection characteristics on the surface of the coating, and the strip and linear defects are probably related to factors such as uneven solution flow or scratches in the coating process. Sorting out the defect types in advance helps to subsequently analyze the corresponding substrate problems for each defect specifically.
[0046] In some embodiments, the size requirements of the coated plate sample are as follows: the length is 5 mm to 10 mm, the width is 5 mm to 10 mm, and the thickness is 0.5 mm to 3 mm.
[0047] In the embodiments of the present application, the size of the coated plate sample can be as follows: the length is 5 mm to 10 mm, the width is 5 mm to 10 mm, and the thickness is 0.5 mm to 3 mm. Appropriate sizes of the coated plate sample are beneficial for subsequent operations. Samples that are too small may be difficult to macroscopically mark the defect positions with a cutter, resulting in a large marking positioning error; while samples that are too large may not fit the sample stage of the focused ion beam equipment, or consume too many reagents in processes such as cleaning and coating removal, increasing costs and operation difficulties. Limiting the size range can ensure the smooth and efficient progress of the analysis process. Exemplarily, in the size of the coated plate sample, the length can be 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, etc.; the width can be 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, etc., and the thickness can be 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, etc.
[0048] In some embodiments, the coated plate sample includes one of the following: galvanized sheet, alloyed galvanized sheet, aluminum-zinc sheet, zinc-aluminum-magnesium sheet.
[0049] In the embodiments of the present application, the coated plate sample can be one of galvanized sheet, alloyed galvanized sheet, aluminum-zinc sheet, zinc-aluminum-magnesium sheet, and tinplate.
[0050] S2. Use the focused ion beam method (FIB) to perform multi-point positioning cutting on the patchy defect positions of the pretreated coated plate sample. The number of cutting points for the multi-point positioning cutting is not less than 3, and the cutting depth of each cutting point is greater than the coating thickness of the coated plate sample;
[0051] S3. Connect each of the cutting points to form a multi-point connection area to obtain the coated plate sample to be analyzed;
[0052] In some embodiments, the size requirements for the cutting points are as follows: the length is 15 μm to 30 μm, and the width is 10 μm to 15 μm.
[0053] In the embodiments of the present application, the focused ion beam method (FIB) is a microfabrication and analysis technique. Its core principle is to generate an ion beam through an ion source, and then use electrostatic lenses and electromagnetic lenses to focus the ion beam onto a tiny area on the surface of the sample. The pre-treated coated plate is subjected to multi-point positioning cutting using the focused ion beam method, and the number of cutting points is not less than 3. In the embodiments of the present application, an FIB-SEM dual-beam system is used, combining the focused ion beam (FIB) technology and the scanning electron microscope (SEM). Compared with single-point cutting, multi-point positioning cutting can more accurately locate the defect area, which is beneficial to more easily and quickly find the position of the patchy defect in the electron beam mode of the scanning electron microscope (SEM); the cutting depth at each cutting point is greater than the coating thickness, which can ensure penetration of the coating and reach the substrate directly, so that whether analyzing the coating surface or the corresponding position of the substrate subsequently, the information obtained is coherent and complete, and the cause of the defect can be accurately explored. The length of the cutting point can be 15 μm to 30 μm, and the width can be 10 μm to 15 μm. Appropriate cutting point sizes are of great significance for accurately positioning patchy defects. If the length of the cutting point is less than 15 μm or the width is less than 10 μm, it may not completely cover the key area of the defect and valuable sample information may be missed; if the length of the cutting point is greater than 30 μm or the width is greater than 15 μm, it may damage too much of the normal coating and substrate tissue, interfere with subsequent microtopography analysis, and make it difficult to accurately judge the cause of the defect. Such a fine definition of the size can ensure that the cutting operation accurately captures the defect without causing excessive damage to the sample. Exemplarily, the length of the cutting point can be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm, 30 μm, etc.; the width can be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, etc.
[0054] In some embodiments, the beam current of the focused ion beam method is 15 nA to 30 nA.
[0055] In the embodiments of the present application, the beam current of the focused ion beam method can be 15 nA to 30 nA. The beam current size is directly related to the cutting efficiency and cutting quality. If the beam current is too small, the cutting speed is slow and a large amount of time cost is consumed; if the beam current is too large, although the cutting speed is fast, it is easy to cause problems such as over-etching and thermal damage to the sample, changing the original microstructure of the sample and making the analysis result distorted. In the range of 15 nA to 30 nA, the cutting speed and sample integrity can be better balanced to ensure that the sample quality in the multi-point connection area meets the strict requirements of subsequent microtopography analysis. Exemplarily, the beam current of the focused ion beam method can be 15 nA, 16 nA, 17 nA, 18 nA, 19 nA, 20 nA, 21 nA, 22 nA, 23 nA, 24 nA, 25 nA, 26 nA, 27 nA, 28 nA, 29 nA, 30 nA, etc.
[0056] S4. Perform microscopic morphology analysis on the multi-point connection area of the to-be-analyzed coated plate sample to obtain a first image;
[0057] In the embodiments of the present application, through the first image, we can see whether the coating morphology is regular, whether there are impurity particles, or whether there are abnormalities such as holes and cracks. For example, if the crystal growth direction of the coating is disordered, it is very likely that parameters such as the composition, temperature, and flow rate of the plating solution deviate during the preparation process, which provides key clues for locking the cause of the defect.
[0058] Exemplarily, S2 to S4 include: fixing the to-be-analyzed sample on the sample stage and placing it in the sample chamber of the FIB dual-beam electron microscope, raising the sample stage to a confocal distance of 7 mm, and then tilting the sample stage to 52°. At this time, the images in the electron beam window and the ion beam window are the same. Move the marked patchy defect sample to the exact middle of the window, and then select a beam current of 15 nA to 30 nA in the ion beam window for rough cutting. The cutting point during rough cutting is rectangular, with dimensions: length 15 μm to 30 μm, width 10 μm to 15 μm, and the depth needs to be set according to the coating thickness. When the coating thickness is about 10 μm, the rough cutting depth can be set to 15 μm to 20 μm. Ensure that the cutting depth is greater than the coating thickness during cutting. In order to accurately locate the position of the patchy defect on the coating surface on the substrate, three points can be selected around the patchy defect for cutting. The connection of these three positions forms a triangle. This method is called the triangular positioning cutting method. At the same time, use the electron beam to perform microscopic morphology analysis on the multi-point connection area, which is the first image, and take a photo and save it.
[0059] S5. Remove the surface coating of the to-be-analyzed coated plate sample to obtain a substrate sample;
[0060] In some embodiments, the stripping solution used for the stripping is a mixed solution of concentrated hydrochloric acid and water.
[0061] In some embodiments, the volume ratio of the concentrated hydrochloric acid to the water is (5 - 10):(5 - 10).
[0062] In the embodiments of the present application, a mixed solution of concentrated hydrochloric acid and water is selected as the stripping solution, which utilizes the chemical reaction between hydrochloric acid and the coating metal. Hydrochloric acid has strong acidity and can react with common coating metals such as zinc and aluminum to dissolve the coating, thereby achieving separation from the substrate. Compared with some stripping methods such as mechanical grinding, the chemical stripping method can better ensure the integrity of the substrate and reduce the physical damage to the microscopic structure of the substrate, creating good conditions for subsequent accurate analysis of the corresponding defect positions on the substrate.
[0063] The volume ratio of concentrated hydrochloric acid to water can be (5 - 10):(5 - 10), that is, concentrated hydrochloric acid and water are roughly mixed in equal amounts. If the proportion of concentrated hydrochloric acid is too high, the acidity of the solution is too strong. While quickly dissolving the coating, it may corrode the substrate excessively, introducing new artificial interference factors and affecting the analysis of the original patchy defects. If the proportion of water is too high, the acidity of the solution is insufficient, which will lead to low efficiency of coating removal, time-consuming and laborious, and slow down the entire analysis process. The method of equal mixing can, while ensuring the removal efficiency, maintain the original state of the substrate to the greatest extent, making the subsequent microscopic morphology analysis results of the substrate more reliable. Exemplarily, the volume ratio of the concentrated hydrochloric acid to water can be 5:6, 5:7, 5:8, 5:9, 5:10, 10:10, 9:10, 8:9, etc. The volume of the stripping solution can be 10 ml - 20 ml. Pour the prepared mixed solution into a beaker, and then put the coated plate sample to be analyzed into the beaker. The zinc layer on the surface of the coated plate reacts chemically with the mixed solution to generate bubbles that continuously float up. When no more bubbles float up, it indicates that the zinc layer has been completely dissolved. At this time, take out the sample with tweezers, clean it with alcohol and dry it.
[0064] S6. Perform microscopic morphology analysis on the multi-point connection area corresponding to the substrate sample to obtain a second image;
[0065] S7. Analyze the reasons for the patchy defects on the coating surface of the coated plate sample according to the first image and the second image.
[0066] In the embodiment of the present application, after removing the coating, analyzing the corresponding position of the substrate forms a perfect complement to the analysis of the coating surface. By comparing the first image and the second image, it is possible to keenly capture whether there is separation, oxidation or other abnormalities at the interface between the coating and the substrate. If the surface of the substrate is rough and uneven at the bonding interface, it is very likely that poor substrate pretreatment affects the adhesion of the coating. On the contrary, if there is impurity accumulation in the coating, it is probably due to insufficient purity of the plating solution.
[0067] Exemplarily, S6 and S7 include: putting the substrate sample with the zinc layer removed into a FIB dual-beam electron microscope, finding the morphology of the corresponding rough cutting position on the substrate at the same magnification, and comparing it with the coated plate sample to be analyzed before removing the zinc layer. Move the sample stage so that the multi-point connection area at the three vertices of the triangle corresponds one by one, and observe and analyze the microscopic morphology of the multi-point connection area of the substrate (the second image) for comparative analysis.
[0068] The analysis method for accurately positioning the substrate with patchy defects on the surface of a coated plate provided by the embodiment of the present application has the following advantages:
[0069] 1. Multi-point positioning: Set no less than 3 cutting points. Obtain local information through single-point cutting. The area formed by connecting multiple cutting points is like a net that can completely "catch" the patchy defect area. Additionally, in the electron beam mode, the position of the defect can be quickly and accurately found. For example, when the patchy defect presents an irregular shape or is scattered, multi-point positioning can ensure that no subtle problem areas are missed and capture the full picture of the defect to the greatest extent. Sufficient cutting depth: Require that the depth of each cutting point is greater than the coating thickness. The coating and the substrate are closely connected upper and lower structures. Only by penetrating the coating and delving into the substrate can we accurately judge whether the defect occurs in the coating or the substrate when analyzing the coating surface and exploring the corresponding position of the substrate later;
[0070] 2. Coating surface analysis (first image), focus on the coating surface in the multi-point connection area formed by the cutting point positions for microscopic morphology analysis, and we can see whether the coating morphology is regular, whether there are impurity particles, or whether there are abnormalities such as holes and cracks. Substrate position analysis (second image), analyze the corresponding position of the substrate after removing the coating, which forms a perfect complement to the coating surface analysis. By comparing the two images, we can keenly capture whether there is separation, oxidation or other abnormalities at the junction of the coating and the substrate. Analyze the cause of the defect by comparing the first image and the second image. Integrate the information obtained comprehensively from the coating to the substrate, from the cross-section to the surface, discard one-sided speculation, and accurately locate whether the defect originates from the coating process, the substrate quality, or the problem of their synergistic effect, so that the subsequent improvement of the coating process and the improvement of product quality can be targeted.
[0071] Generally speaking, the steps of this method cooperate closely, examine the patchy defects of the coated plate from multiple dimensions, improve the accuracy of the analysis of the position of the patchy defects on the coating surface and the corresponding relationship with the substrate, and enhance the accuracy of defect analysis.
[0072] Next, the present application will be further elaborated with specific embodiments. It should be understood that these embodiments are only used to illustrate the present application and not to limit the scope of the present application. The experimental methods without specific conditions noted in the following embodiments are usually determined according to national standards. If there is no corresponding national standard, they are carried out according to general international standards, conventional conditions or the conditions recommended by the manufacturer.
[0073] Example 1
[0074] An analysis method for accurately positioning the substrate of patchy defects on the surface of a coated plate, specifically including:
[0075] S11. Pre-treat the coated plate sample; specifically: the coated plate sample is an alloyed galvanized steel sheet sample with a size of 10 mm in length, 10 mm in width, and 1 mm in thickness. There are obvious patchy defects on its surface, which are visible to the naked eye and appear as irregular white patchy defects. Use a cutter to make macroscopic marks at the positions of the patchy defects, and mark them by scribing, that is, scribe a line with a cutter at the contour edge of the patchy defect to roughly mark the approximate position of the patchy defect. Figure 2 This is a topographical map of the patchy defect with marks on an alloyed galvanized steel sheet sample provided in Embodiment 1 of the present application; please refer to Figure 2 ; Ultrasonically clean the marked alloyed galvanized steel sheet sample with alcohol as the cleaning solution.
[0076] S21. Use the focused ion beam method to perform multi-point positioning cutting on the patchy defect positions of the pre-treated coated plate sample. The number of cutting points for multi-point positioning cutting is 3, and the cutting depth of each cutting point is greater than the coating thickness of the coated plate sample; S31. Connect the lines of each cutting point to form a multi-point connection area to obtain the coated plate sample to be analyzed; S41. Perform microscopic topography analysis on the multi-point connection area of the coated plate sample to be analyzed to obtain the first image; specifically: fix the pre-treated alloyed galvanized steel sheet sample on the sample stage and place it in the FIB dual-beam electron microscope sample chamber. Raise the sample stage to a confocal distance of 7 mm, and then tilt the sample stage to 52°. At this time, the images in the electron beam window and the ion beam window are the same. Move the scribed and marked patchy defect sample to the center of the window, and then select a beam current of 25 nA in the ion beam window for rough cutting. The cutting rectangle size during rough cutting is: 25 μm in length, 15 μm in width, and 20 mm in depth (the coating thickness is 10 μm). Ensure that the cutting depth is greater than the coating thickness during cutting. In addition, to accurately locate the position of the patchy defect on the substrate on the coating surface, select three points around the patchy defect for rough cutting. The multi-point connection area formed by the connection of these three positions is triangular; use the electron beam to perform image analysis on the microscopic topography of the coating surface at the cutting point positions of the patchy defect in the multi-point connection area of the coated plate sample to be analyzed, and take pictures and save them; Figure 3 This is a topographical map of the triangular positioning cutting of the patchy defect on an alloyed galvanized steel sheet sample provided in Embodiment 1 of the present application; please refer to Figure 3 ;
[0077] S51. Remove the surface coating of the coated plate sample to be analyzed to obtain a substrate sample. Specifically, use a mixed solution of concentrated hydrochloric acid and distilled water to remove the zinc layer on the surface of the coated plate. The mixed solution contains 8 ml of concentrated hydrochloric acid and 8 ml of distilled water, and is configured into a 16 ml mixed solution. Pour the configured mixed solution into a beaker, and then place the sample to be analyzed into the beaker. The zinc layer on the surface of the coated plate reacts chemically with the mixed solution to generate bubbles that continuously float upward. When no more bubbles float upward, it indicates that the zinc layer has been completely dissolved. At this time, use tweezers to take out the substrate sample of the alloyed galvanized steel sheet, clean it with alcohol and dry it.
[0078] S61. Analyze the microtopography of the multi-point connection area corresponding to the substrate sample to obtain a second image. Specifically, place the substrate sample with the zinc layer removed into a FIB dual-beam electron microscope. Find the topography of the corresponding rough cutting position on the substrate at the same magnification, and compare it with the photo saved before removing the zinc layer. Move the sample stage so that the cutting positions of the three vertices of the triangle correspond one by one. After verification, observe the microtopography difference on the surface of the substrate, and then take a photo and save it. Figure 4 This is the surface topography diagram of the substrate sample after removing the zinc layer of an alloyed galvanized steel sheet sample provided in Embodiment 1 of the present application; please refer to Figure 4 .
[0079] S71. Analyze the reasons for the patchy defects on the surface of the coating layer of the coated plate sample based on the first image and the second image.
[0080] Cause analysis: Figure 3 (Triangular positioning) is Figure 2 a partial enlarged image of Figure 4 the patchy defect topography on the surface of the substrate after removing the zinc layer. Figure 3 It shows that compared with the normal area, there are fewer holes in the patchy defect area, and the coating layer is relatively flatter; Figure 4 It shows that after pickling, the patchy defect positions on the surface of the substrate correspond one by one to the surface of the coating layer. The relatively flat local area of the patchy defect on the surface of the coating layer corresponds to a rougher or more damaged surface of the substrate at the same position, which causes the coating layer in this local area to be slightly thicker and the alloying to be insufficient, resulting in subsequent patchy defects.
[0081] One or more technical solutions in the embodiments of the present application at least further have the following technical effects or advantages:
[0082] (1) An analysis method for accurately positioning the substrate with patchy defects on the surface of a coated plate provided in the embodiment of the present application has very accurate positioning. After removing the zinc layer, the position of the patchy defect corresponding to the substrate can be quickly located by a scanning electron microscope, so as to find out the specific reasons for the patchy defects on the surface of the coating layer.
[0083] The above are only specific embodiments of the present application, enabling those skilled in the art to understand or implement the present application. Various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown herein, but rather to the broadest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for analyzing the accurate positioning of a substrate with spot-like defects on the surface of a coated plate, the method comprising: The coated plate samples are pretreated; Using a focused ion beam method, multi-point positioning cutting is performed on the spot-like defect position of the pretreated coated plate sample, wherein the number of cutting points of the multi-point positioning cutting is not less than 3, and the cutting depth of each cutting point is greater than the coating thickness of the coated plate sample; Connect each of the cutting points to form a multi-point connection area to obtain a coated plate sample to be analyzed; Performing microscopic morphology analysis on the multi-point connection area of the coated plate sample to be analyzed to obtain a first image; Removing the surface coating of the coated plate sample to be analyzed to obtain a substrate sample; Performing microscopic morphology analysis on the multi-point connection area corresponding to the substrate sample to obtain a second image; According to the first image and the second image, the cause of the spotty defects on the coating surface of the coated plate sample is analyzed.
2. The method according to claim 1, characterized in that The size requirements of the cutting point are as follows: the length is 15 μm to 30 μm, and the width is 10 μm to 15 μm.
3. The method according to claim 1, characterized in that: The beam current of the focused ion beam method is 15nA to 30nA.
4. The method according to claim 1, characterized in that: The removal liquid used in the removal is a mixed solution of concentrated hydrochloric acid and water.
5. The method according to claim 4, characterized in that The volume ratio of the concentrated hydrochloric acid to the water is (5-10):(5-10).
6. The method according to claim 1, characterized in that The coated plate samples include the following: galvanized plate, alloyed galvanized plate, aluminum-zinc plate, and zinc-aluminum-magnesium plate.
7. The method according to claim 1, characterized in that The size requirements of the coated plate sample are as follows: length is 5mm-10mm, width is 5mm-10mm, and thickness is 0.5mm-3mm.
8. The method according to claim 1, characterized in that The spot-like defects include at least one of the following: black spot defects, bright spot defects, strip-like defects, and linear defects.
9. The method according to claim 1, characterized in that: The pretreatment of the coated plate sample comprises: Mark the location of the spot defects on the coated plate sample; The coated plate samples were cleaned after marking.
10. The method according to claim 9, characterized in that The marking method includes one of the following: drawing an arrow, drawing a line, drawing a circle; and / or, The cleaning liquid used for the cleaning includes at least one of the following: alcohol and acetone.