A high-strength vehicle tarpaulin and its preparation method

By introducing a multi-layer structure and specific additives into PVC vehicle tarpaulins, the problem of insufficient tarpaulin strength has been solved, achieving high strength and durability, and ensuring the safety of goods during transportation.

CN120269900BActive Publication Date: 2026-11-10SHIJIAZHUANG WISE TRADING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510658932.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-10
Estimated Expiration
2045-05-21

AI Technical Summary

Technical Problem

Existing PVC vehicle tarpaulins are not strong enough and are easily torn or ripped by cargo during vibration and bumps, causing the cargo to be corroded by rain and dust.

Method used

The structure consists of a first PVC layer, a base fabric layer, and a second PVC layer. The base fabric layer is made of fiberglass mesh or polyester fiber mesh. An adhesive layer is used between the layers. Polyvinyl lactone and composite titanium dioxide are added to the PVC layer. The high-strength tarpaulin is formed by hot pressing and bonding.

Benefits of technology

It significantly improves the tear resistance and peel strength of the tarpaulin, enhances the overall mechanical properties of the tarpaulin, and ensures the integrity of goods during transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of tarpaulin technology, and proposes a high-strength vehicle tarpaulin and its preparation method. The high-strength vehicle tarpaulin includes, from bottom to top, a first PVC layer, a base fabric layer, and a second PVC layer. A first adhesive layer is disposed between the first PVC layer and the base fabric layer, and a second adhesive layer is disposed between the second PVC layer and the base fabric layer. The base fabric layer is made of one of glass fiber mesh, polyester fiber mesh, and PVC mesh. The materials of the first PVC layer and the second PVC layer each independently include the following raw materials in parts by weight: 100 parts PVC resin, 15-20 parts first plasticizer, 20-30 parts calcium powder, 5-8 parts titanium dioxide, 2-3 parts stabilizer, and 5-10 parts polyvinyl lactone glycol. This technical solution solves the problem of low strength in vehicle tarpaulins in related technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field, specifically to a high-strength vehicle tarpaulin and its preparation method. Background Technology

[0002] PVC vehicle tarpaulins consist of a base layer, a PVC layer, and an adhesive layer. PVC material is characterized by its low cost and good waterproof performance. Vehicles experience vibrations during travel and may encounter bumpy roads. The tarpaulin must withstand the impact forces generated by vibrations and collisions of the cargo inside the vehicle. If the tarpaulin is not strong enough, it will be torn or ripped by the cargo, allowing rainwater, dust, and other contaminants to penetrate. Therefore, to ensure the integrity of goods during transportation, the strength of PVC vehicle tarpaulins needs to be increased. Summary of the Invention

[0003] This invention proposes a high-strength vehicle tarpaulin and its preparation method, which solves the problem of low strength of vehicle tarpaulins in related technologies.

[0004] The technical solution of the present invention is as follows: This invention proposes a high-strength vehicle tarpaulin, comprising a first PVC layer, a base fabric layer, and a second PVC layer arranged sequentially from bottom to top. A first adhesive layer is disposed between the first PVC layer and the base fabric layer, and a second adhesive layer is disposed between the second PVC layer and the base fabric layer. The base fabric layer is made of either glass fiber mesh or polyester fiber mesh. The materials of the first PVC layer and the second PVC layer each independently comprise the following raw materials in parts by weight: 100 parts PVC resin, 15-20 parts first plasticizer, 20-30 parts calcium powder, 5-8 parts titanium dioxide, 2-3 parts stabilizer, and 5-10 parts polyethylene glycol.

[0005] As a further technical solution, the stabilizer includes one or more of calcium stearate, zinc stearate, and magnesium stearate.

[0006] During processing and use, tarpaulins are affected by heat, light, etc., which can damage and degrade the PVC molecular structure, forming microscopic defects inside and causing a decrease in the strength of the tarpaulin. The addition of stabilizers can maintain the structural integrity of the PVC molecular chain and maintain the strength of the tarpaulin.

[0007] As a further technical solution, the calcium powder includes one of light calcium carbonate and heavy calcium carbonate.

[0008] As a further technical solution, the thickness of the first adhesive layer and the second adhesive layer are each independently 0.04~0.06mm.

[0009] As a further technical solution, the thickness of the first PVC layer and the first PVC layer are independently 0.3~0.4mm.

[0010] As a further technical solution, the thickness of the base fabric layer is 0.2~0.3mm.

[0011] As a further technical solution, the weight-average molecular weight of the polyvinyl lactone diol is 530~2000.

[0012] As a further technical solution, the polyvinyl lactone diol is composed of a first polyvinyl lactone diol and a second polyvinyl lactone diol, wherein the first polyvinyl lactone diol and the second polyvinyl lactone diol have different weight-average molecular weights.

[0013] As a further technical solution, the weight-average molecular weight of the first polyethylene glycol is 830, the weight-average molecular weight of the second polyethylene glycol is 2000, and the amount of the first polyethylene glycol added is greater than the amount of the second polyethylene glycol added.

[0014] This invention discovers that the addition of polyvinyl lactone (PVC) not only improves the strength of automotive tarpaulins, but also, by compounding PVC with different weight-average molecular weights, the peel strength of the tarpaulin can be further improved. This invention specifies that the weight-average molecular weight of the first PVC is 830 and the weight-average molecular weight of the second PVC is 2000. During the preparation process, the low weight-average molecular weight PVC can fill the gaps between PVC molecules, and also allows the high weight-average molecular weight PVC to be better dispersed and entangled with PVC molecules, thus strengthening the overall mechanical properties. The high weight-average molecular weight PVC can provide a stable network structure for the low weight-average molecular weight PVC. Through the synergistic effect of the interweaving of the low and high weight-average molecular weight PVC, the strength of the tarpaulin can be further improved.

[0015] As a further technical solution, the mass ratio of the first polyvinyl lactone diol to the second polyvinyl lactone diol is 4:1~2.

[0016] In this invention, limiting the ratio of first polyvinyl lactone diol and second polyvinyl lactone diol with different weight-average molecular weights can give full play to their synergistic effect and further improve the strength of the tarpaulin.

[0017] As a further technical solution, the raw materials of the first adhesive layer and the second adhesive layer each independently include the following components by weight: 100 parts PVC paste resin, 20-30 parts second plasticizer, 15-20 parts titanium dioxide, 2-3 parts antioxidant, and 70-80 parts organic solvent.

[0018] As a further technical solution, the titanium dioxide is a composite titanium dioxide, which includes nano-titanium dioxide and amino compounds. The amino compounds include one or more of methyl p-aminobenzoate, methyl 4-amino-3-aminocarbonylbenzoate, and ethyl 3-amino-2,4-diaminomethylbenzoate, preferably methyl 4-amino-3-aminocarbonylbenzoate.

[0019] In this invention, the compatibility between titanium dioxide and PVC paste resin is poor, and titanium dioxide itself has the problem of easy agglomeration. Therefore, after titanium dioxide is modified by composite, the problems of easy agglomeration and poor compatibility can be solved. Moreover, since the PVC layer contains calcium powder and titanium dioxide, the addition of composite titanium dioxide after hot pressing can also improve the peel strength of the tarpaulin.

[0020] In this invention, the selection of amino compounds has a certain impact on the peel strength of the tarpaulin. Compared with the selection of methyl 4-amino-3-aminocarbonylbenzoate as an amino compound, the peel strength of the tarpaulin can be further improved, and the peel strength can reach up to 103N.

[0021] As a further technical solution, the preparation method of the composite titanium dioxide includes the following steps: adding nano-titanium dioxide into a solution and dispersing it evenly, adding an amino compound for improvement, and then drying to obtain composite titanium dioxide.

[0022] As a further technical solution, the amino compound is 3% to 5% of the mass of nano-titanium dioxide, preferably 4%.

[0023] As a further technical solution, the modification temperature is 30~50℃, preferably 40℃, and the modification time is 1~3h, preferably 2h.

[0024] As a further technical solution, the antioxidant includes one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.

[0025] During the processing of PVC paste resin, the PVC slurry is heated. At high temperatures, its molecular chains are unstable and easily generate free radicals under the action of oxygen. These free radicals can trigger chain reactions, leading to the breakage and cross-linking of resin molecular chains, which reduces the performance of PVC paste resin. The addition of antioxidants can capture these free radicals generated under the action of oxygen, terminate the chain reaction, and maintain high bonding performance.

[0026] As a further technical solution, the PVC paste resin includes one or more of PR-457, PR-450, BPR-440, and BPR-450, wherein the degree of polymerization of PR-457 is 800±100, the degree of polymerization of PR-450 is 1000±100, the degree of polymerization of BPR-440 is 1450±200, and the degree of polymerization of BPR-450 is 1000±1000, preferably PR-450, BPR-440, or BPR-450, and more preferably BPR-440.

[0027] As a further technical solution, the organic solvent is cyclohexanone.

[0028] As a further technical solution, the first plasticizer and the second plasticizer each independently include one or more of dioctyl phthalate, diisononyl phthalate, and dioctyl terephthalate.

[0029] In this invention, adding plasticizers to PVC resin can improve intermolecular forces and increase the strength of PVC resin. Adding plasticizers to PVC paste resin can improve fluidity, increase the contact area with the PVC layer surface and the base fabric layer, and improve the peel strength between the PVC layer and the base fabric layer.

[0030] The present invention also proposes a method for preparing a high-strength vehicle tarpaulin, which includes the following steps: hot-pressing and bonding the tarpaulin in the following order from bottom to top: a first PVC layer, a first adhesive layer, a base fabric layer, a second adhesive layer, and a second PVC layer, to obtain the high-strength vehicle tarpaulin.

[0031] The working principle and beneficial effects of this invention are as follows: In this invention, a PVC slurry is used to bond the PVC layer to the base layer. The main components of the PVC slurry are the same as those of the PVC layer; therefore, the PVC slurry and PVC layer have excellent compatibility and exhibit better bonding performance compared to other adhesives. Furthermore, polyvinyl lactone (PEG) is added to the PVC layer. The addition of PEG not only improves the compatibility of calcium powder and titanium dioxide with the PVC resin in the PVC layer, but also makes the calcium powder and titanium dioxide more evenly distributed in the PVC layer, thereby increasing the strength of the PVC automotive tarpaulin. Detailed Implementation

[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0033] In the following embodiments and comparative examples: The base fabric layer is made of PVC mesh fabric, 0.3mm thick, with a 1cm mesh. PVC paste resin: Model BPR-440, Corning Chemicals; PVC resin: S-65, Formosa Plastics Ningbo; Nano titanium dioxide: average particle size 50nm; Light calcium carbonate: average particle size 1250 mesh; Titanium dioxide: average particle size 1250 mesh.

[0034] Example 1 A method for preparing a high-strength vehicle tarpaulin includes the following steps: S1. 100 parts of PVC resin, 15 parts of dioctyl phthalate, 20 parts of light calcium carbonate, 5 parts of titanium dioxide, 2 parts of calcium stearate, and 5 parts of polyethylene glycol are mixed, extruded, and calendered to obtain a PVC film with a thickness of 0.3 mm; wherein the weight average molecular weight of polyethylene glycol is 830. S2. Mix 100 parts of PVC paste resin, 20 parts of dioctyl phthalate, 15 parts of nano titanium dioxide, 2 parts of antioxidant 1010 and 70 parts of cyclohexanone evenly to obtain PVC slurry. S3. After coating the first adhesive layer onto the upper surface of the first PVC layer (coating thickness of 0.04mm) and the lower surface of the second PVC layer (coating thickness of 0.04mm), hot-press bonding is performed in the order of first PVC layer, first adhesive layer, base fabric layer, second adhesive layer, and second PVC layer from bottom to top to obtain a high-strength vehicle tarpaulin; the materials of the first adhesive layer and the second adhesive layer are both PVC slurry prepared in S2, and the materials of the first PVC layer and the second PVC layer are both PVC film with a thickness of 0.3mm.

[0035] Example 2 A method for preparing a high-strength vehicle tarpaulin includes the following steps: S1. 100 parts of PVC resin, 20 parts of dioctyl phthalate, 30 parts of light calcium carbonate, 8 parts of titanium dioxide, 3 parts of calcium stearate, and 10 parts of polyethylene glycol are mixed, extruded, and calendered to obtain a PVC film with a thickness of 0.4 mm; wherein the weight average molecular weight of polyethylene glycol is 830. S2. Mix 100 parts of PVC paste resin, 30 parts of dioctyl phthalate, 20 parts of nano titanium dioxide, 3 parts of antioxidant 1010 and 80 parts of cyclohexanone evenly to obtain PVC slurry. S3. After coating the first adhesive layer onto the upper surface of the first PVC layer (coating thickness of 0.06mm) and the lower surface of the second PVC layer (coating thickness of 0.06mm), hot-press bonding is performed in the order of first PVC layer, first adhesive layer, base fabric layer, second adhesive layer, and second PVC layer from bottom to top to obtain a high-strength vehicle tarpaulin; the materials of the first adhesive layer and the second adhesive layer are both PVC slurry prepared in S2, and the materials of the first PVC layer and the second PVC layer are both PVC films with a thickness of 0.4mm.

[0036] Example 3 The only difference between Example 3 and Example 1 is that the weight-average molecular weight of polyvinyl lactone diol is 2000.

[0037] Example 4 Compared with Example 1, the only difference in Example 4 is that the polyvinyl lactone diol is composed of a first polyvinyl lactone diol (weight average molecular weight of 830) and a second polyvinyl lactone diol (weight average molecular weight of 2000) in a mass ratio of 4:1.5.

[0038] Example 5 Compared with Example 1, the only difference in Example 5 is that the polyvinyl lactone diol is composed of a first polyvinyl lactone diol (weight average molecular weight of 530) and a second polyvinyl lactone diol (weight average molecular weight of 2000) in a mass ratio of 4:1.5.

[0039] Example 6 Compared with Example 1, the only difference in Example 6 is that the polyvinyl lactone diol is composed of a first polyvinyl lactone diol (weight average molecular weight of 830) and a second polyvinyl lactone diol (weight average molecular weight of 3000) in a mass ratio of 4:1.5.

[0040] Example 7 Compared with Example 6, the only difference in Example 7 is that the titanium dioxide in the PVC slurry in Example 7 is composite titanium dioxide. The preparation method of composite titanium dioxide includes the following steps: 40 parts of nano titanium dioxide are added to 300 parts of anhydrous ethanol and dispersed evenly, then 1.6 parts of methyl para-aminobenzoate are added and modified at 40°C for 2 hours, and then dried to obtain composite titanium dioxide.

[0041] Example 8 The only difference between Example 8 and Example 7 is that methyl p-aminobenzoate is replaced with an equal amount of methyl 4-amino-3-aminocarbonylbenzoate.

[0042] Example 9 The only difference between Example 9 and Example 7 is that methyl para-aminobenzoate is replaced with an equal amount of ethyl 3-amino-2,4-diaminomethylbenzoate.

[0043] Example 10 The only difference between Example 10 and Example 8 is that 1.2 parts of methyl 4-amino-3-aminocarbonylbenzoate were used.

[0044] Example 11 The only difference between Example 11 and Example 8 is the addition of 2 parts of methyl 4-amino-3-aminocarbonylbenzoate.

[0045] Comparative Example 1 Compared with Example 1, the only difference in Comparative Example 1 is that polyvinyl lactone (weight-average molecular weight of 830) was not added.

[0046] Experimental Example The tear resistance and peel strength of the vehicle tarpaulins in Examples 1-9 and Comparative Example 1 were determined using the following methods: (1) Tear resistance: The longitudinal tear resistance of the tarpaulin was determined according to the test method in DIN 53363; (2) Peel strength: The peel strength of the tarpaulin was determined according to the test method in FZ / T 60039; (3) Migration resistance: The migration rate of the tarpaulin was determined by the weight loss method. Test conditions: 65℃, 30d; The measurement results are shown in Tables 1-3.

[0047] Table 1. Performance test results of vehicle tarpaulins in Examples 1-6 and Comparative Example 1

[0048] As shown in Table 1, the tear resistance of the tarpaulin in Examples 1 to 6 of this invention is as high as 846 to 935 N, which has excellent tear resistance.

[0049] Table 2 Performance test results of vehicle tarpaulins in Examples 6-11

[0050] As shown in Table 2, the peel strength of the vehicle tarpaulin of the present invention can reach up to 105N, and the addition of composite titanium dioxide can improve the glass strength of the tarpaulin.

[0051] Table 3. Determination of migration performance of vehicle tarpaulin in Example 1

[0052] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A high-strength vehicle tarpaulin, characterized in that, The material comprises, from bottom to top, a first PVC layer, a base fabric layer, and a second PVC layer. A first adhesive layer is disposed between the first PVC layer and the base fabric layer, and a second adhesive layer is disposed between the second PVC layer and the base fabric layer. The base fabric layer is made of one of glass fiber mesh, polyester fiber mesh, and PVC mesh. The raw material for both the first and second adhesive layers is PVC slurry. The materials of the first and second PVC layers each independently comprise the following components by weight: 100 parts PVC resin, 15-20 parts first plasticizer, 20-30 parts calcium powder, 5-8 parts titanium dioxide, 2-3 parts stabilizer, and 5-10 parts polycaprolactone diol. The polycaprolactone diol is composed of a first polycaprolactone diol and a second polycaprolactone diol. The weight-average molecular weight of the first polycaprolactone diol is 830, and the weight-average molecular weight of the second polycaprolactone diol is 2000. The mass ratio of the first polycaprolactone diol to the second polycaprolactone diol is 4:1~2. The raw materials for the first adhesive layer and the second adhesive layer each independently include the following components by weight: 100 parts PVC paste resin, 20-30 parts second plasticizer, 15-20 parts titanium dioxide, 2-3 parts antioxidant, and 70-80 parts organic solvent. The titanium dioxide is a composite titanium dioxide, which includes nano-titanium dioxide and amino compounds.

2. The high-strength vehicle tarpaulin according to claim 1, characterized in that, The thickness of the first adhesive layer and the second adhesive layer are each 0.04~0.06mm.

3. The high-strength vehicle tarpaulin according to claim 1, characterized in that, The thickness of the first PVC layer and the first PVC layer varies independently from 0.3 to 0.4 mm in different regions.

4. The high-strength vehicle tarpaulin according to claim 1, characterized in that, The thickness of the base fabric layer is 0.2~0.3mm.

5. A high-strength vehicle tarpaulin according to claim 1, characterized in that, The amino compounds include one or more of methyl p-aminobenzoate, methyl 4-amino-3-aminocarbonylbenzoate, and ethyl 3-amino-2,4-diaminomethylbenzoate.

6. A high-strength vehicle tarpaulin according to claim 1, characterized in that, The method for preparing the composite titanium dioxide includes the following steps: adding nano-titanium dioxide into a solution and dispersing it evenly, then adding an amino compound for modification, and finally drying to obtain composite titanium dioxide.

7. A high-strength vehicle tarpaulin according to claim 1, characterized in that, The first plasticizer and the second plasticizer each independently include one or more of dioctyl phthalate, diisononyl phthalate, and dioctyl terephthalate.

8. A method for preparing a high-strength vehicle tarpaulin, used to prepare a high-strength vehicle tarpaulin as described in any one of claims 1 to 7, characterized in that, Includes the following steps: The high-strength vehicle tarpaulin is obtained by hot-pressing and bonding the layers in the following order from bottom to top: first PVC layer, first adhesive layer, base fabric layer, second adhesive layer, and second PVC layer.

Citation Information

Patent Citations

  • Degradable PVC plastic

    CN109161128A

  • Ultraviolet-resistant photovoltaic cable

    CN119331322A

  • Tear-resistant PVC (polyvinyl chloride) composite vehicle tarpaulin, equipment, preparation method and application

    CN119567680A