A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel
By controlling the annealing temperature, holding time, and cooling rate in a nitrogen atmosphere, the problem of adjusting the alloying elements of high-performance soft magnetic stainless steel has been solved, resulting in soft magnetic stainless steel with high permeability and ultra-low coercivity, suitable for high-end applications such as high-frequency solenoid valves.
Patent Information
- Application Number
- CN202510200142.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-24
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-02-24
AI Technical Summary
The existing high-performance soft magnetic stainless steel cannot meet the requirements of high permeability and ultra-low coercivity by adjusting the alloying elements. Moreover, the heat treatment process is inefficient and energy-intensive, making it difficult to balance excellent magnetic properties and cost-effectiveness.
Heat treatment is carried out in a nitrogen atmosphere, and the annealing temperature, holding time and cooling rate are controlled. Combined with the gas flow rate of the nitrogen protective atmosphere annealing furnace, the wire rod is ensured to be free of oxidation, obtain a uniform equiaxed crystal structure, reduce coercivity and improve magnetic permeability.
It significantly improves the magnetization and plasticity of soft magnetic stainless steel, achieving high magnetic permeability and ultra-low coercivity, making it suitable for high-end applications such as high-frequency solenoid valves.
Smart Images

Figure CN120272678B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of soft magnetic stainless steel, and in particular to a heat treatment process for soft magnetic stainless steel with high magnetic permeability and ultra-low coercivity. Background Technology
[0002] Soft magnetic materials refer to magnetic materials that can rapidly respond to changes in external magnetic fields and achieve high magnetic flux density with low iron loss. These materials are commonly processed into automatic control components such as solenoid valves, and are widely used in the field of electronic components, with demand continuing to grow. Compared with traditional soft magnetic materials such as silicon steel and pure iron, soft magnetic stainless steel exhibits enormous market potential and application prospects due to its superior magnetic properties and corrosion resistance. Currently, high-performance soft magnetic stainless steel mainly relies on imports, primarily used in high-frequency solenoid valves, which have higher requirements for magnetic properties, including high permeability, low coercivity, and higher saturation magnetic induction. These superior properties make the solenoid valves more sensitive and rapid in response to external magnetic fields, resulting in more advanced equipment. Therefore, developing high-magnetic-induction, ultra-low iron-loss soft magnetic stainless steel for solenoid valves is not only necessary but also advanced, helping to accelerate import substitution and solve bottleneck problems in key areas.
[0003] Key performance indicators of soft magnetic stainless steel include magnetic properties, corrosion resistance, machinability, drawing performance, and weldability. Soft magnetic stainless steel materials used in high-frequency solenoid valves require a balance between soft magnetic properties and ductility. The main factors affecting the soft magnetic properties of ferritic stainless steel are alloy composition and microstructure. For example, Chinese patent application CN115287544B, recently filed by the applicant, discloses a soft magnetic stainless steel wire rod with excellent weldability. This stainless steel wire rod comprises C≤0.020%, Si: 1.50~1.80%, Mn≤0.50%, Cr: 14.0~15.0%, Ni: ≤0.40%, Mo: 0.20~0.40%, N≤0.020%, P<0.020%, S≤0.010%, and Ti: 0. 0.5~0.10%, Nb: 0.20~0.40%, Al: 0.020~0.030%, with the balance being Fe and unavoidable impurities; the manufacturing method includes sequentially passing the furnace charge through electric arc furnace smelting, AOD furnace smelting, LF refining furnace refining, ingot casting, electroslag remelting, rough rolling, high-speed wire rod rolling, solution treatment, and pickling processes; in the solution treatment process, the hot-rolled wire rod formed by high-temperature rolling at above 1050℃ is subjected to solution heat treatment in an annular solution furnace, with the heat treatment temperature being 850~950℃ and the heat treatment time being controlled at more than 60 minutes.
[0004] The existing technical solutions described above have the following drawbacks: While increasing the alloying elements in the stainless steel wire rod improves the material's plasticity, it also increases smelting costs and the difficulty of subsequent processing. Furthermore, adjusting the alloying element content has limited effect on improving magnetic properties, especially in applications requiring high permeability and ultra-low coercivity, where simply adjusting the alloy composition is insufficient to meet practical needs. In addition, although the aforementioned heat treatment process can optimize the material's microstructure and improve soft magnetic properties to some extent, it is often accompanied by high energy consumption, low efficiency, and coarse microstructure, hindering the reduction of industrial production costs and the achievement of plasticity targets. Therefore, how to ensure excellent magnetic properties in soft magnetic stainless steel while simultaneously achieving good plasticity and cost-effectiveness has become a pressing technical challenge. To address this challenge, this invention proposes an innovative heat treatment process. This process aims to achieve high permeability and ultra-low coercivity soft magnetic stainless steel through precise control of heat treatment parameters and optimized alloy composition design, thereby meeting the stringent material performance requirements of high-end applications such as high-frequency solenoid valves. Summary of the Invention
[0005] The problem to be solved by the present invention is to provide a heat treatment process for soft magnetic stainless steel with high permeability and ultra-low coercivity, which addresses the above-mentioned shortcomings of the prior art. This process has the advantages of increasing the maximum permeability of soft magnetic stainless steel, reducing the coercivity of soft magnetic stainless steel, and improving the plasticity index of soft magnetic stainless steel.
[0006] The above-mentioned objective of this invention is achieved through the following technical solutions: A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel includes the following steps: In a nitrogen atmosphere, hot-rolled wire rod is first heated to 900-950℃ at a heating rate of 30-50℃ / h and held for 4-6h to obtain a fine-grained structure of equiaxed recrystallized ferrite. Then, it is cooled to room temperature at a cooling rate of ≤15℃ / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0007] By adopting the above technical solution and using a nitrogen protective atmosphere for heat treatment, oxidation of hot-rolled wire rods at high temperatures can be prevented, thus protecting their surface structure from recrystallization. When the annealing temperature is set at 900~950℃, grain boundaries can completely merge, ensuring complete recrystallization of the internal structure and reducing the proportion of grain boundaries and precipitates. Ideally, the holding time of the annealing process should be maintained at 4~6 hours, which helps to make the wire rod structure more uniform and the grains equiaxed. In addition, by precisely controlling the cooling rate of the wire rod after high-temperature annealing, the internal structure can be homogenized, and stress concentration can be effectively reduced, thereby reducing coercivity and increasing permeability. Furthermore, by adjusting the gas flow rate of the nitrogen protective atmosphere annealing furnace, it can be ensured that the wire rod is free from oxidation, avoiding problems such as local overheating and excessively coarse grains.
[0008] Furthermore, the flow rate of the nitrogen gas is ≥50m³. 3 / h.
[0009] Furthermore, the heating process is carried out in an atmosphere-protected annealing furnace.
[0010] Furthermore, the cooling method is air cooling.
[0011] Furthermore, the soft magnetic stainless steel is composed of the following raw materials in weight percentage: C: ≤0.03%, Si: 1.50~2.00%, Mn: ≤1.0%, P: ≤0.04%, Cr: 15.50~16.50%, Mo: 0.20~0.60%, N: ≤0.03%, with the remainder being Fe and unavoidable impurities.
[0012] Furthermore, the soft magnetic stainless steel is composed of the following raw materials in weight percentage: C: 0.015~0.020%, Si: 1.53~1.58%, Mn: 0.75~0.80%, P: 0.023~0.025%, Cr: 15.60~15.71%, Mo: 0.33~0.37%, N: 0.011~0.013%, with the remainder being Fe and unavoidable impurities.
[0013] Specifically, the soft magnetic stainless steel used in high-frequency solenoid valves is required to have excellent magnetic properties, including saturation magnetic induction intensity ≥1.58T, coercivity ≤180A / m, maximum permeability ≥1800H / m, and remanent magnetic induction intensity ≤0.5T, in order to achieve the high-frequency and precise control requirements of the solenoid valve in application; the role of each chemical component and design principles in this invention are explained below. Carbon (C) and nitrogen (N): C and N are the main forming elements of austenitic stainless steel. As a ferritic stainless steel, soft magnetic stainless steel needs to reduce the austenite content and increase the ferrite content. Therefore, it is necessary to control the C and N content in soft magnetic steel. In this invention, the carbon content is controlled at ≤0.03% and the nitrogen content is controlled at ≤0.03%. Silicon (Si): Silicon is a strong deoxidizer, reducing the oxygen content in steel and improving inclusions. Silicon can increase the permeability of soft magnetic steel and reduce coercivity; therefore, the silicon content in this invention is controlled at 1.50~2.00%. Manganese (Mn): Manganese is an austenite-forming element. Manganese has limited effect on improving magnetic properties, therefore the manganese content in this invention is controlled at ≤0.40%; Phosphorus (P): Phosphorus is a harmful element in steel, causing it to become brittle at cold. In this invention, the phosphorus content is controlled at ≤0.04%. Chromium (Cr): Chromium is the main element in stainless steel. As the chromium content in stainless steel increases, the pitting corrosion sites rise and the corrosion resistance improves. However, excessive chromium will reduce magnetic permeability. Therefore, the chromium content in this invention is controlled at 15.50~16.50%. Molybdenum (Mo): As an important element in austenitic stainless steel, the main function of molybdenum is to improve the corrosion resistance of stainless steel together with chromium, especially to improve the resistance to pitting corrosion and crevice corrosion. Therefore, the molybdenum content in this invention is controlled at 0.20~0.60%.
[0014] Furthermore, the maximum magnetic permeability of the soft magnetic stainless steel is ≥2000H / m, and the coercivity is ≤100A / m.
[0015] Furthermore, the saturation magnetic induction intensity of the soft magnetic stainless steel is ≥1.60T, and the remanent magnetic induction intensity is ≤0.50T.
[0016] Furthermore, the soft magnetic stainless steel has a tensile strength of 450~500MPa, an elongation after fracture of 35.0~40.0%, and a reduction of area of 65.0~70.0%.
[0017] Furthermore, the soft magnetic stainless steel has a grain size of grade 6.
[0018] In summary, the beneficial technical effects of this invention are as follows: By designing the annealing temperature and holding time, and introducing a nitrogen protective atmosphere, the heat treatment process of this invention can significantly increase the recrystallization ratio and reduce the grain boundary ratio of soft magnetic stainless steel. This improvement makes the material more conducive to domain wall movement during magnetization, thus facilitating magnetization and rapid demagnetization. Furthermore, this process significantly improves the overall mechanical properties of the material, ensuring excellent processing performance, and ultimately achieving the goals of increasing the maximum permeability of soft magnetic stainless steel, reducing its coercivity, and improving its plasticity. Attached Figure Description
[0019] Figure 1 This is a hysteresis loop diagram of the soft magnetic stainless steel of Embodiment 1 of the present invention.
[0020] Figure 2 This is a hysteresis loop diagram of the soft magnetic stainless steel of Comparative Example 1 of the present invention.
[0021] Figure 3 This is a metallographic image of the soft magnetic stainless steel of Embodiment 1 of the present invention.
[0022] Figure 4 This is a metallographic image of the soft magnetic stainless steel of Comparative Example 1 of the present invention. Detailed Implementation
[0023] To make the technical means, creative features, objectives and effects of this invention clearer and easier to understand, the invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0024] Example 1: A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel disclosed in this invention includes the following steps: in a nitrogen atmosphere, the nitrogen flow rate is controlled at 60 m³ / s. 3 The process involves first placing hot-rolled wire rod into an atmosphere-protected annealing furnace, heating it to 950°C at a heating rate of 34°C / h, holding it at that temperature for 4.5h to obtain a fine-grained structure of equiaxed recrystallized ferrite, and then cooling it to room temperature at a cooling rate of 13°C / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0025] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.020%, Si: 1.55%, Mn: 0.80%, P: 0.025%, Cr: 15.6%, Mo: 0.33%, N: 0.011%, with the remainder being Fe and unavoidable impurities.
[0026] The soft magnetic stainless steel was tested and found to have a coercivity of 89.7 A / m, a maximum permeability of 2496 H / m, a remanent magnetic induction of 0.4 T, a saturation magnetic induction of 1.63 T, a tensile strength of 461 MPa at room temperature, an elongation after fracture of 37.5%, and a reduction of area of 67%.
[0027] Example 2: A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel disclosed in this invention includes the following steps: in a nitrogen atmosphere, the nitrogen flow rate is controlled at 58 m³ / s. 3 The process involves first placing hot-rolled wire rod into an atmosphere-protected annealing furnace, heating it to 930℃ at a heating rate of 39℃ / h, holding it at that temperature for 5.0h to obtain a fine-grained structure of equiaxed recrystallized ferrite, and then cooling it to room temperature at a cooling rate of 11℃ / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0028] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.019%, Si: 1.58%, Mn: 0.75%, P: 0.023%, Cr: 15.65%, Mo: 0.36%, N: 0.012%, with the remainder being Fe and unavoidable impurities.
[0029] The soft magnetic stainless steel was tested and found to have a coercivity of 92.1 A / m, a maximum permeability of 2110 H / m, a remanent magnetic induction of 0.43 T, a saturation magnetic induction of 1.62 T, a tensile strength of 474 MPa at room temperature, an elongation after fracture of 36.5%, and a reduction of area of 66%.
[0030] Example 3: A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel disclosed in this invention includes the following steps: in a nitrogen atmosphere, the nitrogen flow rate is controlled at 56 m³ / s. 3 The process involves first placing hot-rolled wire rod into an atmosphere-protected annealing furnace, heating it to 900℃ at a heating rate of 41℃ / h, and holding it at that temperature for 5.8h to obtain a fine-grained structure of equiaxed recrystallized ferrite. Then, the wire rod is cooled to room temperature at a cooling rate of 10℃ / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0031] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.015%, Si: 1.53%, Mn: 0.77%, P: 0.024%, Cr: 15.71%, Mo: 0.37%, N: 0.013%, with the remainder being Fe and unavoidable impurities.
[0032] The soft magnetic stainless steel was tested and found to have a coercivity of 98.3 A / m, a maximum permeability of 2073 H / m, a remanent magnetic induction of 0.45 T, a saturation magnetic induction of 1.6 T, a tensile strength of 487 MPa at room temperature, an elongation after fracture of 35.5%, and a reduction of area of 65.5%.
[0033] Example 4: A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel disclosed in this invention includes the following steps: in a nitrogen atmosphere, the nitrogen flow rate is controlled at 50 m³ / s. 3 / h, first put the hot-rolled wire rod into the atmosphere-protected annealing furnace, heat it to 900℃ at a heating rate of 30℃ / h, hold it for 4.0h to obtain a fine-grained structure of equiaxed recrystallized ferrite, and then cool it to room temperature at a cooling rate of 5℃ / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0034] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.010%, Si: 1.50%, Mn: 0.50%, P: 0.020%, Cr: 15.50%, Mo: 0.20%, N: 0.010%, with the remainder being Fe and unavoidable impurities.
[0035] Example 5: A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel disclosed in this invention includes the following steps: in a nitrogen atmosphere, the nitrogen flow rate is controlled at 70 m³ / s. 3 The process involves first placing hot-rolled wire rod into an atmosphere-protected annealing furnace, heating it to 950℃ at a heating rate of 50℃ / h, holding it at that temperature for 6.0h to obtain a fine-grained structure of equiaxed recrystallized ferrite, and then cooling it to room temperature at a cooling rate of 15℃ / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0036] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.030%, Si: 2.00%, Mn: 1.00%, P: 0.040%, Cr: 16.50%, Mo: 0.60%, N: 0.030%, with the remainder being Fe and unavoidable impurities.
[0037] Comparative Example 1: This invention discloses a heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel, which includes the following steps. Without nitrogen protection, hot-rolled wire rod is first placed in an atmosphere-protected annealing furnace and heated to 820°C at a heating rate of 34°C / h, and held at that temperature for 4.0h to obtain a fine-grained structure of equiaxed recrystallized ferrite. Then, it is cooled to room temperature at a cooling rate of 30°C / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0038] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.017%, Si: 1.56%, Mn: 0.78%, P: 0.027%, Cr: 15.77%, Mo: 0.31%, N: 0.020%, with the remainder being Fe and unavoidable impurities.
[0039] The soft magnetic stainless steel was tested and found to have a coercivity of 224 A / m, a maximum permeability of 930 H / m, a remanent magnetic induction of 0.63 T, a saturation magnetic induction of 1.51 T, a tensile strength of 521 MPa at room temperature, an elongation after fracture of 30%, and a reduction of area of 58%.
[0040] The following is a combination Figures 1-4 The properties of the soft magnetic stainless steel prepared in Example 1 and Comparative Example 1 of the present invention are compared.
[0041] in, Figure 1 The hysteresis loop of the soft magnetic stainless steel prepared in Example 1 is shown below. Figure 1 It can be seen that the BH loop has a relatively narrow area, indicating that it has high permeability and ultra-low coercivity. The material can reach saturation when the magnetic field strength is 2000 A / m, and can be demagnetized instantly when the reverse magnetic field strength is 90 A / m. It can meet the market requirements for high frequency and high efficiency solenoid valve cores. Figure 2 The hysteresis loop of the soft magnetic stainless steel prepared in Comparative Example 1 is shown below. Figure 2 It can be seen that the BH loop has a relatively wide area and a relatively flat curve. The material needs to reach saturation when the magnetic field strength is 5000A / m, but the saturation magnetic induction intensity is not high. At the same time, it needs to be demagnetized when the reverse magnetic field strength is 224A / m. The entire magnetization and demagnetization process is relatively slow and cannot meet the requirements of the high-frequency solenoid valve core in the market. Figure 3 The transverse microstructure distribution of the soft magnetic stainless steel prepared in Example 1 is shown below. Figure 3 It can be seen that the room temperature microstructure of Example 1 is equiaxed grains with a high degree of homogenization. There is no coarse ferrite structure and the grain boundaries are clear. Its grain size rating is level 6, which ensures the stability of the material's mechanical properties. Figure 4 To show the transverse microstructure distribution of the soft magnetic stainless steel obtained in Comparative Example 1, from... Figure 4 It can be seen that there are unrecrystallized subgrain structures, and the overall grain size is rated as 7 to 8.
[0042] Based on the above performance test results, and combined with Figures 1-4 It can be found that the high permeability and ultra-low coercivity soft magnetic stainless steel produced by this invention has excellent magnetic properties, with the maximum permeability of the finished material ≥2000 and the coercivity ≤100A / m; the saturation magnetic induction intensity of the finished material ≥1.6T and the remanent magnetic induction intensity ≤0.5T; and excellent plasticity at room temperature, with an elongation of 35.0~40.0% and a reduction of area of 65~70%.
[0043] Therefore, this invention ensures the material achieves complete recrystallization and a uniformly distributed microstructure by setting heat treatment process parameters, including annealing temperature, heating rate, holding time, and cooling rate, and by introducing nitrogen protection measures. This significantly improves the magnetic properties and plasticity of soft magnetic stainless steel. The high permeability and ultra-low coercivity soft magnetic stainless steel produced using this invention's process effectively solves the problems of difficult magnetization and slow disconnection encountered by soft magnetic stainless steel in applications. This type of material is mainly used in the field of high-frequency solenoid valves and has begun to gradually replace imported products.
[0044] Comparative Example 2: This invention discloses a heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel, which includes the following steps. Without nitrogen protection, hot-rolled wire rod is first placed in an atmosphere-protected annealing furnace and heated to 850°C at a heating rate of 34°C / h, and held for 4.0h to obtain a fine-grained structure of equiaxed recrystallized ferrite. Then, it is cooled to room temperature at a cooling rate of 30°C / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0045] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.019%, Si: 1.55%, Mn: 0.71%, P: 0.026%, Cr: 15.83%, Mo: 0.41%, N: 0.011%, with the remainder being Fe and unavoidable impurities.
[0046] The soft magnetic stainless steel was tested and found to have a coercivity of 207 A / m, a maximum permeability of 991 H / m, a remanent magnetic induction of 0.58 T, a saturation magnetic induction of 1.54 T, a tensile strength of 503 MPa at room temperature, an elongation after fracture of 31%, and a reduction of area of 61%.
[0047] Comparative Example 3: This invention discloses a heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel, which includes the following steps. Without nitrogen protection, hot-rolled wire rod is first placed in an atmosphere-protected annealing furnace and heated to 880°C at a heating rate of 34°C / h, and held for 4.0h to obtain a fine-grained structure of equiaxed recrystallized ferrite. Then, it is cooled to room temperature at a cooling rate of 30°C / h to homogenize the ferrite structure and obtain soft magnetic stainless steel.
[0048] The soft magnetic stainless steel is composed of the following raw materials by weight percentage: C: 0.021%, Si: 1.57%, Mn: 0.88%, P: 0.024%, Cr: 15.73%, Mo: 0.39%, N: 0.022%, with the remainder being Fe and unavoidable impurities.
[0049] The soft magnetic stainless steel was tested and found to have a coercivity of 175 A / m, a maximum permeability of 1317 H / m, a remanent magnetic induction of 0.53 T, a saturation magnetic induction of 1.56 T, a tensile strength of 496 MPa at room temperature, an elongation after fracture of 33%, and a reduction of area of 63%.
[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel, characterized in that: The process includes the following steps: In a nitrogen atmosphere, hot-rolled wire rod is first heated to 900-950℃ at a heating rate of 30-50℃ / h and held for 4-6h to obtain a fine-grained structure of equiaxed recrystallized ferrite. Then, it is cooled to room temperature at a cooling rate of ≤15℃ / h to homogenize the ferrite structure and obtain soft magnetic stainless steel. The soft magnetic stainless steel is composed of the following raw materials in weight percentage: C: ≤0.03%, Si: 1.50~2.00%, Mn: ≤1.0%, P: ≤0.04%, Cr: 15.50~16.50%, Mo: 0.20~0.60%, N: ≤0.03%, with the remainder being Fe and unavoidable impurities.
2. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 1, characterized in that: The flow rate of the nitrogen gas is ≥50m³. 3 / h.
3. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 1, characterized in that: The heating process is carried out in an atmosphere-protected annealing furnace.
4. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 1, characterized in that: The cooling method is air cooling.
5. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 1, characterized in that: The soft magnetic stainless steel is composed of the following raw materials in weight percentage: C: 0.015~0.020%, Si: 1.53~1.58%, Mn: 0.75~0.80%, P: 0.023~0.025%, Cr: 15.60~15.71%, Mo: 0.33~0.37%, N: 0.011~0.013%, with the remainder being Fe and unavoidable impurities.
6. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 1, characterized in that: The soft magnetic stainless steel has a maximum permeability of ≥2000H / m and a coercivity of ≤100A / m.
7. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 6, characterized in that: The soft magnetic stainless steel has a saturation magnetic induction intensity ≥1.60T and a residual magnetic induction intensity ≤0.50T.
8. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 6, characterized in that: The soft magnetic stainless steel has a tensile strength of 450~500MPa, an elongation after fracture of 35.0~40.0%, and a reduction of area of 65.0~70.0%.
9. The heat treatment process for high permeability and ultra-low coercivity soft magnetic stainless steel according to claim 6, characterized in that: The soft magnetic stainless steel has a grain size of grade 6.
Citation Information
Patent Citations
A soft magnetic stainless steel wire rod with excellent weldability and its manufacturing method
CN115287544B
Soft-magnetic stainless steel and method for manufacturing soft-magnetic stainless steel wire
CN111471918A
Low-Cr-series soft magnetic stainless steel and control method of structure of low-Cr-series soft magnetic stainless steel