High-temperature reduction flame iron body porcelain and preparation method thereof

By precisely controlling the chemical composition and preparation process of high-temperature reduction flame iron-timber porcelain, the problem of traditional iron-timber porcelain is easily cracked and deformed at high temperatures, achieving the high hardness, heat resistance and unique color of the porcelain body, and improving the overall performance of the porcelain.

CN120329018APending Publication Date: 2025-07-18JINGDEZHEN CERAMICS RESEARCH INSTITUTE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510615484.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2025-07-18

AI Technical Summary

Technical Problem

Traditional iron-tied porcelain is prone to cracking, deformation and other problems in high temperature environments, and the color and texture of the finished product are not ideal.

Method used

By precisely controlling the chemical composition of high-temperature reduction flame iron-titanium porcelain, including specific proportions of silica, aluminum trioxide, all iron and other components, and combining ball milling, filtration, rubbing, firing and other processes, porcelain bodies with high hardness, heat resistance and unique color are prepared.

Benefits of technology

It effectively reduces the cracking and deformation problems of porcelain body in high temperature environments, improves the strength and heat resistance of porcelain body, and maintains unique color and appearance quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120329018A_ABST
    Figure CN120329018A_ABST
Patent Text Reader

Abstract

The invention provides high-temperature reduction flame iron body porcelain and a preparation method thereof, and the iron body porcelain is prepared from the following chemical components in percentage by mass: 66.8 to 72.6 percent of silicon dioxide, 15.5 to 21.7 percent of aluminum oxide, 1.77 to 7.82 percent of total iron, 1.04 to 2.59 percent of magnesium oxide, 0.04 to 1.67 percent of calcium oxide, 0.06 to 0.1 percent of sodium oxide, 1.28 to 3.58 percent of potassium oxide, 0.1 to 0.85 percent of titanium dioxide, 0.02 to 0.03 percent of manganese oxide, 0.02 to 0.15 percent of scale pentoxide and barium oxide. 0.02% of chromium sesquioxide, and 1t of chromium sesquioxide; 0.006%, the content of nickel is 1t; the aluminum alloy comprises the following components in percentage by weight: 0.002% of aluminum, 0.002%-0.003% of copper, 0.006%-0.008% of strontium and 0.02% of zirconium, and the ignition loss is 4.05%-8.42%. According to the high-temperature reduction flame iron body porcelain and the preparation method thereof, the chemical composition is accurately controlled, so that the high-temperature reduction flame iron body porcelain has good physical and chemical properties, and meanwhile, a porcelain body is endowed with relatively high hardness and heat resistance; due to the proper iron content, the porcelain body has unique color and luster, the strength of the porcelain body is enhanced, and the problems of cracking, deformation and the like are effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of porcelain, and particularly relates to a high-temperature reducing-flame iron-core porcelain and a preparation method thereof. Background Art

[0002] In the field of ceramic manufacturing, iron-core porcelain has attracted much attention due to its unique texture and properties. Traditional iron-core porcelain has certain limitations in chemical composition and preparation process, resulting in difficulties in meeting modern diverse requirements in terms of strength, heat resistance, appearance, etc. For example, some iron-core porcelain is prone to cracking, deformation, etc. in high-temperature environments due to unreasonable chemical composition; or due to imperfect preparation processes, the color and texture of the finished products are not ideal enough. Summary of the Invention

[0003] The purpose of the present invention is to provide a high-temperature reducing-flame iron-core porcelain to solve the problems that existing iron-core porcelain is prone to cracking, deformation, etc. in high-temperature environments.

[0004] The present invention provides a high-temperature reducing-flame iron-core porcelain, and its chemical composition includes: calculated by mass percentage, silicon dioxide 66.8 - 72.6%, aluminum oxide 15.5 - 21.7%, total iron 1.77 - 7.82%, magnesium oxide 1.04 - 2.59%, calcium oxide 0.04 - 1.67%, sodium oxide 0.06 - 0.1%, potassium oxide 1.28 - 3.58%, titanium dioxide 0.1 - 0.85%, manganese oxide 0.02 - 0.03%, phosphorus pentoxide 0.02 - 0.15%, barium oxide <0.02%, chromium sesquioxide <0.006%, nickel <0.002%, copper 0.002 - 0.003%, strontium 0.006 - 0.008%, zirconium 0.02%, loss on ignition 4.05 - 8.42%.

[0005] Furthermore, it also includes sulfur trioxide 0.01 - 0.02%, vanadium 0 - 0.01%, zinc 0 - 0.01%.

[0006] Furthermore, the expansion coefficient of the high-temperature reducing-flame iron-core porcelain is: 5 - 7×10-6 / °C.

[0007] The present invention also provides a preparation method of a high-temperature reducing-flame iron-core porcelain, with raw material ratio;

[0008] Ball-mill the proportioned raw materials and then screen them to obtain raw material powders;

[0009] Add the raw material powders into a filter press, add water and then perform filter pressing treatment to obtain a mud-like raw material;

[0010] Knead the mud-like raw material repeatedly to remove the air in the mud-like raw material to obtain a roughly kneaded raw material;

[0011] After placing the rough refining principle for a preset time, knead it repeatedly again to obtain the refined raw material;

[0012] After shaping the refined raw material into the product shape, fire it to obtain the finished product.

[0013] Furthermore, the method of shaping the refined raw material into the product shape and then firing it includes:

[0014] Draw the refined raw material into a blank and trim the formed blank;

[0015] After replenishing water to the trimmed blank, perform a drying treatment on the blank;

[0016] After performing a bisque firing on the dried blank, apply glaze;

[0017] Perform a glaze firing on the glazed blank to obtain the finished product.

[0018] Furthermore, the trimming method includes trimming the whole blank and turning the blank.

[0019] Furthermore, after the step of performing a glaze firing on the glazed blank to obtain the finished product, the method further includes:

[0020] Inspect the finished product.

[0021] Furthermore, the raw materials are 40% of the first iron ore, 5% of the second iron ore, 38% of the kaolin washed mud, and 17% of the Yiyang porcelain stone;

[0022] The chemical composition of the first iron ore includes: 60.1% of silicon dioxide, 20.31% of aluminum oxide, 11.23% of total iron, 1.2% of calcium oxide, 0.34% of magnesium oxide, 2.18% of potassium oxide, 0.82% of sodium oxide, and 4.72% of loss on ignition;

[0023] The chemical composition of the second iron ore includes: 65.28% of silicon dioxide, 19.25% of aluminum oxide, 7.43% of total iron, 0.56% of calcium oxide, 0.83% of magnesium oxide, 1.52% of potassium oxide, 0.95% of sodium oxide, and 4.16% of loss on ignition;

[0024] The chemical composition of the kaolin washed mud includes: 50.95% of silicon dioxide, 35.62% of aluminum oxide, 1.94% of total iron, 0.42% of calcium oxide, 0.24% of magnesium oxide, 1.21% of potassium oxide, 0.38% of sodium oxide, and 9.23% of loss on ignition;

[0025] The chemical composition of Yiyang porcelain stone includes: silicon dioxide 71.99%, aluminum oxide 13.85%, total iron 3.28%, calcium oxide 0.48%, magnesium oxide 0.51%, potassium oxide 2.36%, sodium oxide 0.96%, and loss on ignition 6.57%.

[0026] The above high-temperature reducing flame iron tire porcelain and its preparation method have good physical and chemical properties by precisely controlling the chemical composition. The reasonable combination of components such as silicon dioxide and aluminum oxide endows the porcelain body with high hardness and heat resistance; the appropriate iron content not only gives the porcelain body a unique color but also enhances the strength of the porcelain body, effectively reducing the occurrence of problems such as cracking and deformation. Brief Description of the Drawings

[0027] Figure 1 It is a flow chart of the preparation method of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0028] Figure 2 It is the first sample diagram of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0029] Figure 3 It is the second sample diagram of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0030] Figure 4 It is the third sample diagram of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0031] Figure 5 It is the fourth sample diagram of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0032] Figure 6 It is the fifth sample diagram of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0033] Figure 7 It is the sixth sample diagram of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention;

[0034] Figure 8 It is the sample test report of the high-temperature reducing flame iron tire porcelain in the embodiment of the present invention.

[0035] The following specific embodiments will further illustrate the present invention in conjunction with the above-mentioned drawings. Specific Embodiments

[0036] To facilitate the understanding of the present invention, the present invention will be described more comprehensively below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0037] It should be noted that when an element is referred to as "fixed to" another element, it can be directly on the other element or there may also be an intermediate element. When an element is considered to be "connected" to another element, it can be directly connected to the other element or there may be an intermediate element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used in this article are only for illustrative purposes.

[0038] Unless otherwise defined, all technical and scientific terms used in this article have the same meaning as those commonly understood by those skilled in the technical field to which this invention belongs. The terms used in the specification of this invention are only for the purpose of describing specific embodiments and are not intended to limit this invention. The term "and / or" used in this article includes any and all combinations of one or more of the related listed items.

[0039] Example 1

[0040] The present invention provides a high-temperature reducing flame iron-core porcelain. Please refer to Figures 2 to 8 , and its chemical composition includes: by mass percentage, 66.8% of silicon dioxide, 15.5% of aluminum oxide, 7.82% of total iron, 1.04% of magnesium oxide, 0.04% of calcium oxide, 0.06% of sodium oxide, 3.58% of potassium oxide, 0.85% of titanium dioxide, 0.02% of manganese oxide, 0.15% of phosphorus pentoxide, <0.02% of barium oxide, 0.006% of chromium sesquioxide, <0.002% of nickel, 0.003% of copper, 0.006% of strontium, 0.02% of zirconium, 0.02% of sulfur trioxide, 0.01% of vanadium, 0.01% of zinc, and the loss on ignition is 4.05%.

[0041] For the above high-temperature reducing flame iron-core porcelain, by precisely controlling the chemical composition, it has good physical and chemical properties. The reasonable combination of components such as silicon dioxide and aluminum oxide endows the porcelain body with high hardness and heat resistance; the appropriate iron content not only makes the porcelain body have a unique color but also enhances the strength of the porcelain body. In addition, the stable coefficient of expansion ensures the reliability of the porcelain body in a temperature-changing environment and effectively reduces the occurrence of problems such as cracking and deformation.

[0042] It should be noted that in the embodiments of the present invention, the loss on ignition refers to the mass loss of the ore after being burned at a specified temperature (such as 1200°C commonly used for kaolin, and different ores have different requirements) for a certain period of time due to reasons such as water evaporation, carbon dioxide escape, and organic matter decomposition. Taking kaolin as an example, at high temperatures, the structural water contained in it and the carbon dioxide generated by the decomposition of carbonates will escape, resulting in a reduction in mass.

[0043] Example 2

[0044] An embodiment of the present invention also provides a high-temperature reducing flame iron core porcelain, and its chemical composition includes: by mass percentage, silicon dioxide 72.6%, aluminum oxide 11.7%, total iron 1.77%, magnesium oxide 2.59%, calcium oxide 1.67%, sodium oxide 0.1%, potassium oxide 1.28%, titanium dioxide 0.1%, manganese oxide 0.03%, phosphorus pentoxide 0.02%, barium oxide <0.02%, chromium sesquioxide <0.005%, nickel <0.002%, copper 0.002%, strontium 0.008%, zirconium 0.02%, sulfur trioxide 0.01%, loss on ignition 8.42%.

[0045] For the above high-temperature reducing flame iron core porcelain, by precisely controlling the chemical composition, it has good physical and chemical properties. The reasonable combination of components such as silicon dioxide and aluminum oxide endows the porcelain body with high hardness and heat resistance; the appropriate iron content not only gives the porcelain body a unique color, but also enhances the strength of the porcelain body. In addition, the stable expansion coefficient ensures the reliability of the porcelain body in a temperature-changing environment, effectively reducing the occurrence of problems such as cracking and deformation.

[0046] Specifically, through the above component ratio, the expansion coefficient of the high-temperature reducing flame iron core porcelain is: 5 - 7×10-6 / °C, which is the same as that of traditional Jingdezhen porcelain, so it matches well with the glaze, does not crack, does not peel off the glaze, and improves the thermal shock resistance of the product.

[0047] Example 3

[0048] Please refer to Figure 1 , an embodiment of the present invention also provides a preparation method of a high-temperature reducing flame iron core porcelain, and the method includes;

[0049] Step S01, ball-mill and then screen the proportioned raw materials to obtain raw material powder;

[0050] Step S02, add the raw material powder into a filter press, add water and then perform filter press treatment to obtain a mud-like raw material;

[0051] Step S03, repeatedly knead the mud-like raw material to remove the air in the mud-like raw material to obtain a roughly kneaded raw material;

[0052] Step S04, place the roughly kneaded raw material for a preset time and then knead it repeatedly to obtain a refined raw material;

[0053] Step S05, shape the refined raw material into a product shape and then fire it to obtain a finished product.

[0054] The above-mentioned preparation method of high-temperature reducing flame iron-core porcelain precisely controls the chemical composition, endowing it with good physical and chemical properties. The reasonable combination of components such as silica and alumina gives the porcelain body higher hardness and heat resistance. The appropriate iron content not only makes the porcelain body have a unique color but also enhances the strength of the porcelain body, effectively reducing the occurrence of problems such as cracking and deformation.

[0055] In an embodiment of the present invention, the method of firing the refined raw materials after shaping them into product shapes includes:

[0056] Drawing and shaping the refined raw materials, and trimming the formed blank.

[0057] After replenishing water to the trimmed blank, the blank is dried. During the trimming process, the surface of the blank may become dry. Use tools such as a brush to dip water and apply it on the surface of the blank to make the moisture of the blank uniform, prevent cracking, and also prepare for subsequent processes. Place the trimmed blank in a suitable environment and let it dry slowly until the moisture completely evaporates, so that there will be no problems such as cracking due to the presence of water during firing.

[0058] After the dried blank is bisque-fired, it is glazed. Put the dried blank into a kiln and fire it at a certain temperature. This firing is without glazing, mainly to preliminarily sinter the blank and increase its strength, laying a foundation for glazing and final firing. After the bisque-fired blank cools, the glaze is evenly applied to the surface of the blank by methods such as dipping, spraying, and brushing. The glaze is like a beautiful coat for the porcelain, making the surface of the porcelain smoother, more lustrous, and having a certain protective effect.

[0059] The glazed blank is fired to obtain the finished product. The glazed blank is put into the kiln again and fired at a higher and more appropriate temperature. At high temperature, the glaze will melt and tightly combine with the blank, finally forming a beautiful porcelain appearance.

[0060] In an embodiment of the present invention, the trimming method includes trimming the whole blank and turning the blank. Trimming the whole blank means that the shape of the drawn blank may not be regular and perfect enough, and the craftsman will use tools to further trim it to make its shape, thickness, etc. more in line with the design requirements. Turning the blank means using a special tool to further finely process the trimmed blank to make the outer shape of the blank smoother and the size more precise. This step can make the porcelain look more delicate.

[0061] In an embodiment of the present invention, after the step of firing the glazed blank to obtain the finished product, the method further includes:

[0062] Inspect the finished product. After taking the fired porcelain out of the kiln, carefully check its appearance for defects such as cracks, spots, deformation, etc., and also check whether its dimensions, functions, etc. meet the requirements. Those that meet the standards are finished products.

[0063] For the preparation method of the above-mentioned high-temperature reducing flame iron tire porcelain, put the prepared raw materials into a ball mill. There are many small steel balls in the ball mill. After it rotates, the small steel balls will continuously impact and grind the raw materials, grinding them into fine powders, which will be more convenient for subsequent processing. The ground powders may not be of uniform fineness. Sieve them with a sieve to remove the too coarse particles and leave the uniform and delicate raw material powders to ensure the stable quality of the porcelain produced. Mix the sieved raw material powders with water to form a slurry. It is not okay if there is too much water in the slurry. Use a filter press to squeeze out the excess water in the slurry to make it into a mud block (mud-shaped raw material) with a certain shape and hardness. Knead the filtered mud block repeatedly by machine or by hand to make the mud material more uniform and expel as much air as possible inside. Place the kneaded mud material in a relatively closed and humid place for a period of time, such as one week. This process can make the water in the mud material more uniform and its properties more stable, just like fermenting food materials, making subsequent processing easier to operate. Knead the aged mud material again to further improve the uniformity and fineness of the mud material and make it reach an ideal state suitable for shaping. Place the refined mud material on a potter's wheel. The potter's wheel rotates quickly, and the craftsman skillfully squeezes and stretches the mud material with his hands to slowly make it into the desired porcelain shape, such as various shapes like bowls and bottles. The shape of the pulled blank may not be regular and perfect enough. The craftsman will use tools to trim it again (i.e., trimming the blank) to make its shape, thickness, etc. more in line with the design requirements. Use a special tool to further finely process the trimmed blank to make the outer shape of the blank smoother and the dimensions more accurate. This step can make the porcelain look more delicate (i.e., the process of trimming the embryo).

[0064] In an embodiment of the present invention, the raw materials are 40% of the first iron ore, 5% of the second iron ore, 38% of the kaolin washed mud, and 17% of the Yiyang porcelain stone;

[0065] The chemical composition of the first iron ore includes: 60.1% of silicon dioxide, 20.31% of aluminum oxide, 11.23% of total iron, 1.2% of calcium oxide, 0.34% of magnesium oxide, 2.18% of potassium oxide, 0.82% of sodium oxide, and 4.72% of loss on ignition;

[0066] The chemical composition of the second iron ore includes: 65.28% of silicon dioxide, 19.25% of aluminum oxide, 7.43% of total iron, 0.56% of calcium oxide, 0.83% of magnesium oxide, 1.52% of potassium oxide, 0.95% of sodium oxide, and 4.16% of loss on ignition;

[0067] The chemical composition of the kaolin washing mud includes: silicon dioxide 50.95%, aluminum oxide 35.62%, total iron 1.94%, calcium oxide 0.42%, magnesium oxide 0.24%, potassium oxide 1.21%, sodium oxide 0.38%, and ignition loss 9.23%.

[0068] The chemical composition of the Yiyang porcelain stone includes: silicon dioxide 71.99%, aluminum oxide 13.85%, total iron 3.28%, calcium oxide 0.48%, magnesium oxide 0.51%, potassium oxide 2.36%, sodium oxide 0.96%, and ignition loss 6.57%.

[0069] It should be noted that since the iron content of iron-body porcelain is generally relatively high, crystal form transformation is likely to occur at high temperatures. Therefore, most iron-body porcelain has a relatively narrow firing range, and it is prone to deformation and edge collapse during firing at high temperatures. In this project, by utilizing the mineral advantages of the first iron ore and the second iron ore and optimizing the formula, a unique formula with high temperature resistance and a relatively wide firing range is formed. The product does not deform after firing, and the crystal form transformation is small, thus meeting the various functional requirements of the porcelain body for large-scale production to meet the future needs of large-scale production.

[0070] The above-described embodiments merely represent several implementation manners of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the present invention patent. It should be pointed out that for those of ordinary skill in the art, without departing from the concept of the present invention, several modifications and improvements can still be made, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the appended claims.

Claims

1. A high-temperature reducing flame iron-body porcelain, characterized in that, Its chemical composition includes: by mass percentage, silica 66.8 - 72.6%, aluminum oxide 15.5 - 21.7%, total iron 1.77 - 7.82%, magnesium oxide 1.04 - 2.59%, calcium oxide 0.04 - 1.67%, sodium oxide 0.06 - 0.1%, potassium oxide 1.28 - 3.58%, titanium dioxide 0.1 - 0.85%, manganese oxide 0.02 - 0.03%, phosphorus pentoxide 0.02 - 0.15%, barium oxide <0.02%, chromium sesquioxide <0.006%, nickel <0.002%, copper 0.002 - 0.003%, strontium 0.006 - 0.008%, zirconium 0.02%, and loss on ignition 4.05 - 8.42%.

2. The high-temperature reducing flame iron-core porcelain according to claim 1, wherein It also includes sulfur trioxide 0.01 - 0.02%, vanadium 0 - 0.01%, and zinc 0 - 0.01%.

3. A preparation method of high-temperature reducing flame iron tire porcelain, characterized in that Raw material ratio; The proportioned raw materials are ball milled and then sieved to obtain raw material powder; The raw material powder is added to a filter press, water is added, and then filter pressing treatment is carried out to obtain a mud-like raw material; The mud-like raw material is kneaded repeatedly to remove the air in the mud-like raw material to obtain a roughly kneaded raw material; The roughly kneaded raw material is placed for a preset time and then kneaded repeatedly again to obtain a refined raw material; The refined raw material is shaped into a product shape and then fired to obtain a finished product.

4. The preparation method of the high-temperature reducing flame iron-core porcelain according to claim 3, characterized in that, The method of firing after shaping the refined raw material into a product shape includes: The refined raw material is drawn into shape and the formed blank is trimmed; After the trimmed blank is replenished with water, the blank is dried; The dried blank is subjected to bisque firing and then glazed; The glazed blank is subjected to glaze firing to obtain a finished product.

5. The preparation method of the high-temperature reducing flame iron-core porcelain according to claim 4, characterized in that, The trimming method includes trimming the blank and turning the blank.

6. The preparation method of the high-temperature reducing flame iron tire porcelain according to claim 4, characterized in that, After the step of subjecting the glazed blank to glaze firing to obtain a finished product, the method further includes: Inspecting the finished product.

7. The preparation method of the high-temperature reducing flame iron-core porcelain according to claim 3, characterized in that, The raw materials are 40% of the first iron ore, 5% of the second iron ore, 38% of kaolin washed mud, and 17% of Yiyang porcelain stone; The chemical composition of the first iron ore includes: silica 60.1%, aluminum oxide 20.31%, total iron 11.23%, calcium oxide 1.2%, magnesium oxide 0.34%, potassium oxide 2.18%, sodium oxide 0.82%, and loss on ignition 4.72%; The chemical composition of the second iron ore includes: silica 65.28%, aluminum oxide 19.25%, total iron 7.43%, calcium oxide 0.56%, magnesium oxide 0.83%, potassium oxide 1.52%, sodium oxide 0.95%, and loss on ignition 4.16%; The chemical composition of kaolin washed mud includes: silica 50.95%, aluminum oxide 35.62%, total iron 1.94%, calcium oxide 0.42%, magnesium oxide 0.24%, potassium oxide 1.21%, sodium oxide 0.38%, and loss on ignition 9.23%; The chemical composition of Yiyang porcelain stone includes: silicon dioxide 71.99%, aluminum oxide 13.85%, total iron 3.28%, calcium oxide 0.48%, magnesium oxide 0.51%, potassium oxide 2.36%, sodium oxide 0.96%, and loss on ignition 6.57%.