Polyolefin grafting modification method

By introducing graft polymer brushes on the surface of polyolefin powder, the problem of poor polarity on the surface of polyolefin is solved, the interface bonding force with other materials is improved, and an environmentally friendly and efficient modification method is achieved, which is suitable for industrial production.

CN120329485AActive Publication Date: 2025-07-18NANJING TECH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510518255.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-24
Publication Date
2025-07-18
Estimated Expiration
2045-04-24

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the surface polarity of polyolefins, resulting in weak interface bonding with adhesives, coatings, inks and other materials. The traditional modification methods have problems such as chemical pollution, complex and expensive treatment equipment, low grafting rate and high temperature reactions.

Method used

Using water as a solvent, the surface of the polyolefin powder is modified by light-induced grafting, and a transition metal chloride catalyst, a water-soluble organic reducing agent and a non-ionic emulsifier are used to introduce graft monomers. The reaction conditions are mild, forming a graft polymer brush to enhance the surface polarity.

Benefits of technology

The adhesion between the polyolefin surface and other materials is improved, and the modification effect is energy-saving and environmentally friendly. It is suitable for industrial production, with a grafting rate of 5 to 20 wt%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120329485A_ABST
    Figure CN120329485A_ABST
Patent Text Reader

Abstract

The invention discloses a grafting modification method of polyolefin, which is used for carrying out light-induced grafting modification on chlorinated polyolefin, effectively improving the problem of poor surface polarity of the polyolefin and improving the interface bonding force between the polyolefin and other materials. The method comprises the following steps: 1) removing impurities on the surface of polyolefin powder; 2) preparing chlorinated polyolefin powder; and (3) adding deionized water into a reaction kettle, adding the chlorinated polyolefin powder, introducing nitrogen for 0.5 hour, sequentially adding a transition metal chloride catalyst, a water-soluble organic reducing agent, a non-ionic emulsifier and a grafting monomer in a nitrogen atmosphere, turning on an LED lamp, reacting at the temperature of 15-50 DEG C for more than 5 hours, filtering a reaction solution after the reaction is finished, and drying to obtain the chlorinated polyolefin. And cleaning the obtained filter cake with deionized water, and drying to obtain the grafted modified polyolefin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for modifying polyolefins, and more particularly to a method for graft-modifying polyolefins. Background Art

[0002] Polyolefins are a class of high-molecular materials polymerized from olefin monomers. They are the plastics with the largest global production and the widest application, accounting for more than half of the total global plastic production, and the market scale is still further expanding. However, the simple C-C and C-H structures of polyolefins determine their non-polar and low surface energy chemical inertness. Its surface free energy is only about 30 mN / m, and the liquid contact angle > 90°. It is difficult to adhere to adhesives, coatings, inks, etc. during use, and the interfacial bonding force with other materials is weak. Therefore, effectively improving the surface polarity of polyolefins is a key problem that needs to be solved urgently at home and abroad. At present, at home and abroad, polyolefins are mainly modified by means such as strong acid etching, plasma treatment, chemical grafting, and melt grafting. However, they have problems such as serious chemical pollution, short treatment time, complex and expensive treatment equipment, low grafting rate, and easy gelation; in addition, traditional graft-modification methods also require the use of a large amount of organic solvents as solvents, and more need to carry out reactions under high-temperature conditions, which does not meet the requirements of energy conservation and environmental protection. Therefore, it is necessary to develop a modification method for polyolefins with long-term modification, energy conservation and environmental protection, and mild conditions. Summary of the Invention

[0003] In view of the problems and deficiencies of the prior art, the present invention provides a method for graft-modifying polyolefins. This method grafts a polymer brush on the surface of polyolefin powder in the case of using water as a solvent, effectively improving the problem of poor surface polarity of polyolefins and enhancing the interfacial bonding force between polyolefins and other materials.

[0004] The present invention is realized through the following technical solutions:

[0005] The method for graft-modifying polyolefins of the present invention includes the following steps:

[0006] 1) Cleaning the polyolefin powder with deionized water to remove impurities on the surface of the polyolefin powder, and obtaining pretreated polyolefin powder;

[0007] 2) Preparing a sodium hypochlorite solution, dropping hydrochloric acid into it to adjust the pH to 4-8, adding the pretreated polyolefin powder, irradiating with a xenon lamp, taking out the polyolefin powder after reacting for more than 0.5 h, and cleaning it with deionized water to obtain chlorinated polyolefin powder;

[0008] 3) Add deionized water into the reactor, put in the chlorinated polyolefin powder, after purging with nitrogen for 0.5 h, then under a nitrogen atmosphere, successively add the transition metal chloride catalyst, water-soluble organic reducing agent, non-ionic emulsifier, grafting monomer, turn on the LED lamp, and react at a temperature of 15 - 50 °C for more than 5 hours. After the reaction ends, filter the reaction solution, and the obtained filter cake is washed with deionized water and dried to obtain the graft-modified polyolefin.

[0009] For the above graft-modification method of polyolefin of the present invention, a further technical solution is that the wavelength of the LED lamp is 350 nm - 410 nm.

[0010] For the above graft-modification method of polyolefin of the present invention, a further technical solution may also be that the polyolefin is polypropylene, polyethylene or propylene-ethylene copolymer; the transition metal chloride catalyst is one or a combination of copper bromide, copper chloride, iron bromide, iron chloride, ruthenium bromide, ruthenium chloride, cobalt bromide, cobalt chloride; the water-soluble organic reducing agent is one or a combination of pentamethyldiethylenetriamine, glucose, ethylenediamine, sodium citrate, ascorbic acid; the non-ionic emulsifier is one or a combination of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyglycerol fatty acid ester, sorbitan fatty acid monoesters, polyoxyethylene sorbitan fatty acid monoesters; the grafting monomer is one or a combination of acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, diacetone acrylamide, N-(hydroxymethyl)acrylamide, acrylamide. A further technical solution is that for the fatty alcohol polyoxyethylene ether, the long-chain alkyl R = 12 - 18 and the polyoxyethylene ether group n = 15 - 30; for the fatty acid polyoxyethylene ester, the long-chain alkyl R = 12 - 18 and the polyoxyethylene ether group n = 15 - 30; for the polyglycerol fatty acid ester, the polyglycerol n = 8 - 15; for the sorbitan fatty acid monoesters, the long-chain alkyl R = 12; for the polyoxyethylene sorbitan fatty acid monoesters, the long-chain alkyl R = 12.

[0011] For the above graft-modification method of polyolefin of the present invention, a further technical solution may also be that in step 3), the water-soluble concentration of the transition metal chloride catalyst is 50 ppm - 300 ppm; the water-soluble concentration of the water-soluble organic reducing agent is 200 ppm - 3000 ppm; the dosage of the non-ionic emulsifier is 0.1 - 3 wt% of the deionized water; the dosage of the grafting monomer is 1 - 10 wt% of the deionized water; the chlorinated polyolefin powder is 5 - 30 wt% of the deionized water.

[0012] The structural formula of the graft-modified polyolefin prepared by the above graft-modification method of polyolefin of the present invention is:

[0013]

[0014] In the structural formula, Mn is a grafted polymer, x and y are the degrees of polymerization of the structural units, and the grafting rate is 5-20 wt%.

[0015] The present invention has the following beneficial effects compared with the prior art:

[0016] In the present invention, chlorinated polyolefin is obtained by chlorinating polyolefin, and then, using water as a solvent, transition metal chloride as a catalyst, and organic amine as a reducing agent, photoinduced graft modification of the chlorinated polyolefin is carried out, effectively improving the problem of poor adhesion between the surface of polyolefin products and adhesives, coatings, inks, etc., and improving the compatibility of polyolefin alloy materials. This method is energy-saving and environmentally friendly, and is conducive to realizing industrial production; the reaction conditions of this method are mild, and polyolefin can be modified at room temperature; this method can effectively improve the problem of chemical inertness on the surface of polyolefin, increase the polarity of the polyolefin surface, and improve the problem of poor adhesion between it and adhesives, coatings, inks, etc. Description of the Drawings

[0017] Figure 1 It is a schematic diagram of the reaction process of polyethylene grafted with 2-hydroxyethyl methacrylate monomer Detailed Embodiments

[0018] The preparation method of the chlorinated polyolefin powder in the examples is as follows

[0019] 1) Wash the polyolefin powder with deionized water to remove impurities on the surface of the polyolefin powder, and obtain the pretreated polyolefin powder;

[0020] 2) Prepare a sodium hypochlorite solution and add hydrochloric acid dropwise to adjust the pH to 4-8, add the pretreated polyolefin powder, irradiate with a xenon lamp, after reacting for more than 0.5 h, take out the polyolefin powder, and wash it with deionized water to obtain the chlorinated polyolefin powder;

[0021] At the same time, the graft monomer is pretreated, and the steps are as follows: Carry out vacuum distillation on the graft monomer to remove the inhibitor in the polyolefin powder.

[0022] Example 1

[0023] Add 8 L of deionized water to the reaction kettle, add 200 ml of sodium hypochlorite solution (active chlorine ≥ 5.2%), add hydrochloric acid dropwise to adjust the pH to 4, add the pretreated polyethylene powder, irradiate with a xenon lamp, after reacting for more than 0.5 h, take out the polyethylene powder after the chlorination reaction, and wash it with deionized water to obtain the chlorinated polyethylene powder. Table 1 shows the XPS element content on the surface of the chlorinated polyethylene powder.

[0024] Table 1

[0025]

[0026] Example 2

[0027] Add 8 L of deionized water into a reaction kettle, add 250 ml of sodium hypochlorite solution (active chlorine ≥ 5.2%), add hydrochloric acid dropwise to adjust the pH to 6, add pretreated polypropylene powder, irradiate with a xenon lamp, after reacting for more than 0.5 h, take out the polypropylene powder after chlorination reaction, wash it with deionized water to obtain chlorinated polypropylene powder.

[0028] Example 3

[0029] Add 8 L of deionized water into a reaction kettle, add 220 ml of sodium hypochlorite solution (active chlorine ≥ 5.2%), add hydrochloric acid dropwise to adjust the pH to 5, add pretreated polyethylene-propylene copolymer powder, irradiate with a xenon lamp, after reacting for more than 0.5 h, take out the polyethylene-propylene copolymer powder after chlorination reaction, wash it with deionized water to obtain chlorinated polyethylene-propylene copolymer powder.

[0030] Example 4

[0031] Add 8 L of deionized water into a reaction kettle, purge with nitrogen for 0.5 h; weigh 80 g of 2-hydroxyethyl methacrylate, 0.5 g of cuprous bromide, 2.0 g of pentamethyldiethylenetriamine, 10 g of steareth-21 (fatty alcohol polyoxyethylene ether, R = 18, n = 21), and add them into deionized water in turn under nitrogen protection, stir for 5 min to mix evenly; weigh 400 g of chlorinated polypropylene powder, add it into the reaction solution mixed evenly in the above step under nitrogen protection, turn on the 410 nm ultraviolet lamp, control the reaction temperature at 40 °C for constant temperature, react for 6 h; filter the reaction solution by suction, and the obtained filter cake is the modified polypropylene grafted with poly(2-hydroxyethyl methacrylate), and the grafting rate is 5-6%.

[0032] Example 5

[0033] Add 8 L of deionized water into a reaction kettle, purge with nitrogen for 0.5 h; weigh 400 g of acrylamide, 2.0 g of cuprous chloride, 15 g of pentamethyldiethylenetriamine, 100 g of steareth-20 (fatty alcohol polyoxyethylene ether, R = 18, n = 20), and add them into deionized water in turn under nitrogen protection, stir for 5 min to mix evenly; weigh 1600 g of chlorinated polyethylene powder, add it into the reaction solution mixed evenly in the above step under nitrogen protection, turn on the 365 nm ultraviolet lamp, react at room temperature for 5 h; filter the reaction solution by suction, and the obtained filter cake is the modified polyethylene grafted with polyacrylamide, and the grafting rate is 8-10%.

[0034] Example 6

[0035] Add 8 L of deionized water into the reaction kettle and purge with nitrogen for 0.5 h; weigh 600 g of diacetone acrylamide, 2.0 g of cuprous chloride, and 20 g of glucose, and add them into the deionized water successively under nitrogen protection, and stir for 5 min to mix evenly; weigh 2400 g of chlorinated polyethylene powder, and add it into the reaction solution mixed evenly in the above step under nitrogen protection. Turn on the 365 nm ultraviolet lamp and react at room temperature for 5 h; filter the reaction solution by suction, and the obtained filter cake is the modified polyethylene grafted with polyacrylamide, and the grafting rate is 5-8%.

[0036] Example 7

[0037] Add 8 L of deionized water into the reaction kettle and purge with nitrogen for 0.5 h; weigh 200 g of glycidyl methacrylate, 1.5 g of cobalt bromide, 5.0 g of ethylenediamine, and 5.0 g of ascorbic acid, and add them into the deionized water successively under nitrogen protection, and stir for 5 min to mix evenly; weigh 2000 g of chlorinated polypropylene powder, and add it into the reaction solution mixed evenly in the above step under nitrogen protection. Turn on the 365 nm ultraviolet lamp and react at room temperature for 5 h; filter the reaction solution by suction, and the obtained filter cake is the modified polypropylene grafted with polyacrylamide, and the grafting rate is 6-8%.

[0038] Example 8

[0039] Add 8 L of deionized water into the reaction kettle and purge with nitrogen for 0.5 h; weigh 200 g of glycidyl methacrylate, 2.0 g of ferric bromide, 8.0 g of ethylenediamine, and 15.0 g of PEG-20 stearate (fatty acid polyoxyethylene ester, R = 18, n = 20), and add them into the deionized water successively under nitrogen protection, and stir for 5 min to mix evenly; weigh 1000 g of chlorinated polyethylene powder, and add it into the reaction solution mixed evenly in the above step under nitrogen protection. Turn on the 410 nm ultraviolet lamp and react at 40 °C for 5 h; filter the reaction solution by suction, and the obtained filter cake is the modified polyethylene grafted with polyacrylamide, and the grafting rate is 10-12%.

[0040] Example 9

[0041] Add 8 L of deionized water to the reaction kettle and purge with nitrogen for 0.5 h; weigh 200 g of glycidyl methacrylate, 100 g of methyl methacrylate, 2.0 g of cuprous chloride, 8.0 g of pentamethyldiethylenetriamine, 10 g of PEG-20 stearate (fatty acid polyoxyethylene ester, R = 18, n = 22) and 15 g of Tween-20 (polyoxyethylene sorbitan fatty acid monoesters, R = 12), and add them to the deionized water successively under nitrogen protection, and stir for 5 min to mix evenly; weigh 1800 g of ethylene-propylene copolymer powder, and add it to the reaction solution mixed evenly in the above step under nitrogen protection, turn on the 410 nm ultraviolet lamp, and react at room temperature for 5 h; filter the reaction solution by suction, and the obtained filter cake is the modified ethylene-propylene copolymer grafted with polyacrylamide, and the grafting rate is 15-17%.

Claims

1. A method for graft modification of polyolefin, characterized in that, It includes the following steps: 1) Clean the polyolefin powder with deionized water to remove the impurities on the surface of the polyolefin powder, and obtain the pretreated polyolefin powder; 2) Prepare a sodium hypochlorite solution, add hydrochloric acid dropwise to adjust the pH to 4-8, add the pretreated polyolefin powder, irradiate with a xenon lamp, take out the polyolefin powder after reacting for more than 0.5 h, and wash it with deionized water to obtain the chlorinated polyolefin powder; 3) Add deionized water to the reaction kettle, put in the chlorinated polyolefin powder, pass nitrogen for 0.5 h, and then, under a nitrogen atmosphere, sequentially add a transition metal chloride catalyst, a water-soluble organic reducing agent, a non-ionic emulsifier, and a grafting monomer, turn on the LED lamp, and react at a temperature of 15-50 °C for a reaction time of more than 5 hours. After the reaction is completed, filter the reaction solution, and the obtained filter cake is washed with deionized water and dried to obtain the graft-modified polyolefin.

2. The graft modification method of polyolefin according to claim 1, characterized in that, The wavelength of the LED lamp described is 350 nm - 410 nm.

3. The graft modification method of polyolefin according to claim 1, characterized in that, The polyolefin is polypropylene, polyethylene or propylene-ethylene copolymer; the transition metal chloride catalyst is one or a combination of copper bromide, copper chloride, iron bromide, iron chloride, ruthenium bromide, ruthenium chloride, cobalt bromide, cobalt chloride; the water-soluble organic reducing agent is one or a combination of pentamethyldiethylenetriamine, glucose, ethylenediamine, sodium citrate, ascorbic acid; the non-ionic emulsifier is one or a combination of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyglycerol fatty acid ester, sorbitan fatty acid monoesters, polyoxyethylene sorbitan fatty acid monoesters; the grafting monomer is one or a combination of acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, diacetone acrylamide, N-(hydroxymethyl)acrylamide, acrylamide.

4. The graft modification method of polyolefin according to claim 3, characterized in that For the fatty alcohol polyoxyethylene ether, the long-chain alkyl R = 12-18 and the polyoxyethylene ether group n = 15-30; for the fatty acid polyoxyethylene ester, the long-chain alkyl R = 12-18 and the polyoxyethylene ether group n = 15-30; for the polyglycerol fatty acid ester, the polyglycerol n = 8-15; for the sorbitan fatty acid monoesters, the long-chain alkyl R = 12; for the polyoxyethylene sorbitan fatty acid monoesters, the long-chain alkyl R = 12.

5. The graft modification method of polyolefin according to claim 1, characterized in that, In step 3), the water-soluble concentration of the transition metal chloride catalyst is 50 ppm - 300 ppm; the water-soluble concentration of the water-soluble organic reducing agent is 200 ppm - 3000 ppm; the dosage of the non-ionic emulsifier is 0.1-3 wt% of the deionized water; the dosage of the grafting monomer is 1-10 wt% of the deionized water; the chlorinated polyolefin powder is 5-30 wt% of the deionized water.

6. A graft-modified polyolefin prepared by the graft-modification method of the polyolefin as described in claims 1-5, and its structural formula is: In the structural formula, Mn is the graft polymer, x and y are the polymerization degrees of the structural units, and the grafting rate is 5-20 wt%.

Citation Information

Patent Citations

  • Polymer prepared by polymerization of light-induced active radicals in miniemulsion and process of polymer

    CN104151463A

  • Surface modification method for polyolefin material

    CN109679129A

  • Polyolefin material with surface grafted polymer and preparation method and application of polyolefin material

    CN110698598A

  • Preparation method of chlorinated polypropylene ternary graft

    CN116478335A