High-frequency and high-speed copper-clad plate and manufacturing method thereof

Through the combination of modified resin and modified spherical filler, the problem of poor viscosity of high-frequency and high-speed copper clad resin is solved, the production efficiency and dielectric performance are improved, and efficient copper clad manufacturing is achieved.

CN120396460APending Publication Date: 2025-08-01CHANGZHOU CUIZHENG COMPOSITE MATERIALS TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410127843.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2025-08-01

AI Technical Summary

Technical Problem

The resin viscosity of existing high-frequency high-speed copper clad plates is poor, affecting production efficiency and performance.

Method used

The ratio of modified resin, modified spherical filler and modified reinforcement materials is adopted to reduce the curing reaction temperature by combining polyphenyl ether with bisphenol A cyanate resin prepolymer and bisphenyl epoxy resin, and introduce silicon oxide, boron oxide, sodium oxide, potassium oxide and barium oxide to improve the acid and alkali resistance and spherical properties of the glass.

Benefits of technology

The amount of resin is significantly reduced, the production operation conditions are improved, the production efficiency is improved, and the resin viscosity is maintained at a high addition amount, which improves dielectric performance and overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120396460A_ABST
    Figure CN120396460A_ABST
Patent Text Reader

Abstract

The invention discloses a high-frequency and high-speed copper-clad plate and a manufacturing method thereof.The high-frequency and high-speed copper-clad plate comprises a copper-clad plate body, the copper-clad plate body is manufactured through the steps of burdening, curing, cutting, pre-stacking combination and hot press molding, and the manufactured materials comprise modified resin, modified spherical filler, modified reinforcing material and accelerant; the raw materials are proportioned in parts by weight as follows: 50-60 parts of modified resin, 8-15 parts of modified spherical filler, 8-14 parts of a modified reinforcing material and 5-15 parts of an accelerant; the invention relates to the technical field of high-frequency high-speed copper-clad plates. According to the high-frequency and high-speed copper-clad plate and the manufacturing method thereof, silicon oxide and boron oxide are used as basic components of the low-dielectric spherical filler, sodium oxide and potassium oxide are introduced at the same time, the acid and alkali resistance of glass is improved, the glass melting temperature is reduced by introducing barium oxide, the spheroidizing effect is obvious, the sphericity degree can generally reach 0.950 or above, and the high-frequency and high-speed copper-clad plate is suitable for large-scale production. The flowability is good, and the use amount of the resin can be greatly reduced in the subsequent use process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-frequency and high-speed copper clad laminates, and specifically relates to a high-frequency and high-speed copper clad laminate and a manufacturing method thereof. Background Art

[0002] Referring to a Chinese patent on a manufacturing method of a high-frequency and high-speed copper clad laminate (Publication No.: CN107234851B), a low molecular weight polyphenylene ether and a bisphenol A cyanate resin are blended and modified to prepare a modified PPO / CE resin; the modified PPO / CE resin, a filler, a flame retardant, etc. are processed and mixed in a certain proportion to formulate a special glue for producing high-frequency and high-speed copper clad laminates; then the reinforcing material is pretreated; then the pretreated NE fiberglass cloth and the PPO / CE resin are prepared into a prepreg in an impregnator through units such as pre-impregnation, impregnation, exhaust, and drying; the prepared prepregs are stacked alternately, and the stacked prepregs and a high-frequency and ultra-low friction electrolytic copper foil (VLP) are assembled into a laminate, and then hot-pressed and formed under high temperature and high pressure in a hot press. The high-frequency and high-speed copper clad laminate produced by this method can meet other performance requirements of the copper clad laminate under the condition of reducing the dielectric constant and the dielectric dissipation factor, but the viscosity of the resin is poor and has not been improved accordingly. For this reason, the present invention proposes a high-frequency and high-speed copper clad laminate and a manufacturing method thereof to solve the above-mentioned problems. Summary of the Invention

[0003] (1) Technical Problems to be Solved

[0004] In view of the deficiencies of the prior art, the present invention provides a high-frequency and high-speed copper clad laminate and a manufacturing method thereof, which solve the problems mentioned in the above background art.

[0005] (2) Technical Solutions

[0006] To achieve the above object, the present invention is realized through the following technical solutions: A high-frequency and high-speed copper clad laminate includes a copper clad laminate body, and the copper clad laminate body is made through steps of batching, curing, cutting, pre-stacking combination, and hot pressing and forming, and the materials used include a modified resin, a modified spherical filler, a modified reinforcing material, and a promoter, and are proportioned by weight as follows: 50 - 60 parts of the modified resin, 8 - 15 parts of the modified spherical filler, 8 - 14 parts of the modified reinforcing material, and 5 - 15 parts of the promoter.

[0007] Preferably, the specific preparation method of the modified resin is: First, weigh a certain amount of a bisphenol A cyanate ester resin prepolymer and polyphenylene ether and blend them, then add an appropriate amount of methyl ethyl ketone to dissolve them, and after they are completely dissolved, add a certain weight ratio of a biphenyl type epoxy resin.

[0008] Preferably, the weight ratio of the bisphenol A cyanate ester resin prepolymer, polyphenylene ether, biphenyl type epoxy resin, and methyl ethyl ketone is 1:1:1:0.4.

[0009] Preferably, the specific preparation method of the modified spherical filler is as follows:

[0010] (1) Melt the glass raw materials, then perform water quenching and drying.

[0011] (2) Crush and grind the dried glass raw materials to obtain glass particles with a certain particle size.

[0012] (3) Then put the glass particles into the spheroidizing furnace for reheating, so that the molten glass particles are spheroidized under the action of surface tension.

[0013] (4) Then quickly cool and collect to obtain the modified spherical filler.

[0014] Preferably, the glass raw materials in step (1) include the following components in mass ratio: 72% silica, 19% boron oxide, 4.5% sodium oxide, 2.5% potassium oxide, 1% barium oxide, and 1% others.

[0015] Preferably, the specific treatment method of the modified reinforcing material is as follows:

[0016] 1) Fire the NE fiberglass cloth at 40°C for 30 minutes, and then naturally cool to room temperature.

[0017] 2) Then immerse the heat-treated NE fiberglass cloth in the treatment liquid for 10 - 18 minutes, and naturally air dry for 30 - 40 minutes.

[0018] 3) Then place it in a drying oven at 100°C and dry for 2 hours.

[0019] A manufacturing method of a high-frequency and high-speed copper clad laminate, characterized in that it specifically includes the following steps:

[0020] S1. Take raw materials in proportion and set aside.

[0021] S2. Put the modified resin and accelerator into a high-shear reaction kettle and stir for 5 - 8 hours.

[0022] S3. While stirring, add the modified spherical filler, and then stir at high speed for 2 - 4 hours to obtain glue.

[0023] S4. Coat the surface of the modified reinforcing material with the glue prepared in step S3, and then bake in a drying oven for 8 - 10 minutes to make a prepreg.

[0024] S5. Cut the prepreg obtained in step S4, then stack the cut prepregs neatly together. After reaching an appropriate stacking height, cover copper foils on its upper and lower surfaces, and then put it into a vacuum hot press for hot pressing and forming.

[0025] Preferably, the thickness of the copper foil in step S5 is 9 μm.

[0026] Preferably, the temperature in the vacuum hot press in step S5 is 135 - 230 °C, the pressure is 80 - 450 N, and the pressing time is 4 hours.

[0027] (III) Beneficial effects

[0028] The present invention provides a high-frequency and high-speed copper clad laminate and its manufacturing method. Compared with the prior art, it has the following beneficial effects:

[0029] (1). For the high-frequency and high-speed copper clad laminate and its manufacturing method, adding polyphenylene ether to the bisphenol A cyanate ester resin prepolymer / biphenyl-type epoxy resin system can reduce the curing reaction temperature of the system. This is mainly because polyphenylene ether has the characteristic of catalyzing the reaction of the bisphenol A cyanate ester resin prepolymer, which can accelerate the curing reaction of the bisphenol A cyanate ester resin prepolymer.

[0030] (2). For the high-frequency and high-speed copper clad laminate and its manufacturing method, using silicon oxide and boron oxide as the basic components of the low-dielectric spherical filler, and introducing sodium oxide and potassium oxide at the same time, improves the acid and alkali resistance of the glass. And introducing barium oxide reduces the glass melting temperature. The spheroidization effect is obvious, and the sphericity can generally reach above 0.950, with good fluidity. During subsequent use, the resin dosage can be greatly reduced. Even under the premise of high addition amount, the resin viscosity will not increase much, improving the production operation conditions and significantly increasing the production efficiency. Description of the drawings

[0031] Figure 1 It is the scanning electron microscope picture of the glass particles of the present invention;

[0032] Figure 2 It is the polarized light microscope picture of the glass particles of the present invention. Specific embodiments

[0033] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative efforts belong to the protection scope of the present invention.

[0034] Please refer to Figure 1 - Figure 2, the embodiments of the present invention provide the following three technical solutions:

[0035] Embodiment 1:

[0036] A high-frequency and high-speed copper clad laminate includes a copper clad laminate body, which is made by steps of batching, curing, cutting, pre-laminating combination and hot pressing molding, and the materials used include modified resin, modified spherical filler, modified reinforcing material and accelerator, and are proportioned by weight as follows: 50 g of modified resin, 8 g of modified spherical filler, 8 g of modified reinforcing material and 5 g of accelerator.

[0037] In the embodiment of the present invention, the specific preparation method of the modified resin is as follows: First, a certain amount of bisphenol A cyanate ester resin prepolymer and polyphenylene ether are weighed and blended, then an appropriate amount of methyl ethyl ketone is added to dissolve it, and after it is completely dissolved, a biphenyl-type epoxy resin is added according to a certain weight ratio.

[0038] In the embodiment of the present invention, the bisphenol A cyanate ester resin prepolymer, polyphenylene ether, biphenyl-type epoxy resin and methyl ethyl ketone are in a weight ratio of 1:1:1:0.4.

[0039] Among them, the reaction formula of polyphenylene ether and biphenyl-type epoxy resin is:

[0040]

[0041] Among them, the reaction formula of bisphenol A cyanate ester resin prepolymer and biphenyl-type epoxy resin is:

[0042]

[0043] By adding polyphenylene ether to the bisphenol A cyanate ester resin prepolymer / biphenyl-type epoxy resin system, the curing reaction temperature of the system can be reduced. This is mainly because polyphenylene ether has the characteristic of catalyzing the reaction of bisphenol A cyanate ester resin prepolymer, and can accelerate the curing reaction of bisphenol A cyanate ester resin prepolymer.

[0044] In the embodiment of the present invention, the specific preparation method of the modified spherical filler is as follows:

[0045] (1). Melting the glass raw materials at a melting temperature of 1475 °C, then quenching with water and drying, and the clarification temperature is 1480 °C;

[0046] (2). Crushing and grinding the dried glass raw materials to obtain glass particles with a certain particle size;

[0047] (3). Then putting the glass particles into the spheroidizing furnace for reheating, so that the molten glass particles are spheroidized under the action of surface tension;

[0048] (4) Then, rapidly cool and collect to obtain the modified spherical filler with a dielectric constant of 5.35.

[0049] Sphericity test: The morphology of glass particles is shown in the scanning electron microscope and polarized light microscope photos as Figure 1 、 Figure 2 shown.

[0050] Take the modified spherical filler and characterize it with a BT-2900 dynamic image particle size and particle shape analysis system (wet method) equipment. This equipment takes photos of 10,000 particles through a camera and compares them with the standard atlas of spheres to display the statistical data of the sphericity of the particles. The results are shown in the following table:

[0051]

[0052]

[0053] In the embodiment of the present invention, the glass raw materials in step (1) include the following components by mass ratio: 72% of silicon oxide, 19% of boron oxide, 4.5% of sodium oxide, 2.5% of potassium oxide, 1% of barium oxide, and 1% of others.

[0054] The contents of silicon oxide and boron oxide exceed 90%, which are the most important components of the glass formula. Individually, the dielectric constants of silicon oxide and boron oxide are relatively low. The dielectric constant of fused quartz is 3.8, and that of boron oxide glass is 3.2. However, the melting temperature of silicon oxide is relatively high. Appropriate introduction of boron oxide glass makes melting easier, the integrity of the glass network structure is better, the polarization degree is reduced, and the dielectric constant becomes smaller. At the same time, by controlling the introduction amount, the acid and alkali resistance of the glass is improved, thereby improving its physical and chemical properties. By adding sodium oxide and potassium oxide, sodium ions and potassium ions are introduced, which mainly play a role in breaking the network, have the functions of assisting melting at high temperatures, accelerating glass melting, and significantly reducing hardness. At the same time, the mixed alkali effect will occur between the two alkali metals, resulting in an extremely low value of the dielectric constant. Among the alkaline earth metals, barium has the largest atomic number, the largest ionic radius, and the strongest alkalinity. Therefore, it has a series of characteristics such as improving the refractive index, dispersion, radiation protection, and fluxing of the glass. Barium oxide belongs to a typical network modifier. Its position in the structure and its effect on properties are between alkaline earth metals and alkali metal ions, and it can significantly increase the dielectric constant. By introducing a small amount, it can reduce the high-temperature viscosity of the glass and the glass melting temperature, which is beneficial to industrial production.

[0055] In the embodiment of the present invention, the specific treatment method of the modified reinforcing material is as follows:

[0056] 1) Fire the NE glass fiber cloth at a temperature of 40 °C for 30 minutes, and then naturally cool it to room temperature;

[0057] 2), then immerse the heat-treated NE fiberglass cloth in the treatment liquid for 10 minutes and air-dry it naturally for 30 minutes;

[0058] 3), then place it in a drying oven at 100 °C and dry it for 2 hours.

[0059] A method for manufacturing a high-frequency and high-speed copper clad laminate, characterized in that it specifically includes the following steps:

[0060] S1. Take raw materials in proportion and set aside;

[0061] S2. Put the modified resin and the accelerator into a high-shear reactor and stir for 5 hours;

[0062] S3. Then add the modified spherical filler while stirring, and then stir at high speed for 2 hours to obtain glue;

[0063] S4. Coat the surface of the modified reinforcing material with the glue prepared in step S3, and then bake it in a drying oven for 8 minutes to make a prepreg;

[0064] S5. Cut the prepreg obtained in step S4, then stack the cut prepregs neatly together. After reaching an appropriate stacking height, cover copper foils on its upper and lower surfaces, and then put it into a vacuum hot press for hot pressing and forming.

[0065] In the embodiment of the present invention, the thickness of the copper foil in step S5 is 9 μm.

[0066] In the embodiment of the present invention, the temperature in the vacuum hot press in step S5 is 135 °C, the pressure is 80 N, and the pressing time is 4 hours.

[0067] Dielectric constant and dielectric loss test: Take a copper clad laminate of 2 cm * 2 cm * 2 cm, place it in a polytetrafluoroethylene tube with an outer diameter of 3.2 cm and an inner diameter of 2.8 cm for testing. Connect the reentrant coaxial cavity to a vector network analyzer. After turning on the machine and preheating for 60 min; perform cavity calibration; place the sample to be tested into the reentrant coaxial cavity for testing. The results are as follows in the table:

[0068]

[0069] Example 2:

[0070] A high-frequency and high-speed copper clad laminate, including a copper clad laminate body, which is made by steps of batching, curing, cutting, pre-laminating combination and hot pressing and forming, and the materials used include modified resin, modified spherical filler, modified reinforcing material and accelerator, and are proportioned by the following weight parts: 55 g of modified resin, 12 g of modified spherical filler, 11 g of modified reinforcing material and 10 g of accelerator.

[0071] In the embodiment of the present invention, the specific preparation method of the modified resin is as follows: First, weigh a certain amount of bisphenol A cyanate ester resin prepolymer and polyphenylene ether, blend them, add an appropriate amount of methyl ethyl ketone to dissolve them, and after complete dissolution, add a biphenyl-type epoxy resin in a certain weight ratio.

[0072] In the embodiment of the present invention, the weight ratio of the bisphenol A cyanate ester resin prepolymer, polyphenylene ether, biphenyl-type epoxy resin, and methyl ethyl ketone is 1:1:1:0.4.

[0073] In the embodiment of the present invention, the specific preparation method of the modified spherical filler is as follows:

[0074] (1) Melt the glass raw materials, then perform water quenching and drying.

[0075] (2) Crush and grind the dried glass raw materials to obtain glass particles with a certain particle size.

[0076] (3) Then put the glass particles into the spheroidizing furnace for reheating, so that the molten glass particles are spheroidized under the action of surface tension.

[0077] (4) Then quickly cool and collect to obtain the modified spherical filler.

[0078] In the embodiment of the present invention, the glass raw materials in step (1) include the following components in mass ratio: 72% silica, 19% boron oxide, 4.5% sodium oxide, 2.5% potassium oxide, 1% barium oxide, and 1% others.

[0079] In the embodiment of the present invention, the specific treatment method of the modified reinforcing material is as follows:

[0080] 1) Bake the NE glass fiber cloth at a temperature of 40°C for 30 minutes, and then naturally cool to room temperature.

[0081] 2) Then immerse the heat-treated NE glass fiber cloth in the treatment liquid for 10 minutes and air-dry it naturally for 35 minutes.

[0082] 3) Then place it in a drying oven at 100°C and dry it for 2 hours.

[0083] A manufacturing method of a high-frequency and high-speed copper clad laminate, characterized in that it specifically includes the following steps:

[0084] S1. Take raw materials in proportion and set aside.

[0085] S2. Put the modified resin and accelerator into a high-shear reactor and stir for 7 hours.

[0086] S3. Then add the modified spherical filler while stirring, and then stir at high speed for 3 hours to obtain glue.

[0087] S4. Coat the surface of the modified reinforcing material with the glue prepared in step S3, and then bake it in a drying oven for 9 minutes to make a prepreg;

[0088] S5. Cut the prepreg obtained in step S4, then stack the cut prepregs neatly together. After reaching an appropriate stacking height, cover copper foils on its upper and lower surfaces, and then put it into a vacuum hot press for hot pressing and forming.

[0089] In the embodiment of the present invention, the thickness of the copper foil in step S5 is 9 μm.

[0090] In the embodiment of the present invention, the temperature in the vacuum hot press in step S5 is 185 °C, the pressure is 260 N, and the pressing time is 4 hours.

[0091] Example 3:

[0092] A high-frequency and high-speed copper clad laminate includes a copper clad laminate body, and the copper clad laminate body is made by steps of batching, curing, cutting, pre-laminating combination and hot pressing and forming. The materials used include a modified resin, a modified spherical filler, a modified reinforcing material and a promoter, and are proportioned by the following weight parts: 60 g of modified resin, 15 g of modified spherical filler, 14 g of modified reinforcing material and 15 g of promoter.

[0093] In the embodiment of the present invention, the specific preparation method of the modified resin is as follows: First, weigh a certain amount of bisphenol A cyanate ester resin prepolymer and polyphenylene ether and blend them, then add an appropriate amount of methyl ethyl ketone to dissolve it. After it is completely dissolved, add a certain weight ratio of biphenyl type epoxy resin.

[0094] In the embodiment of the present invention, the weight ratio of bisphenol A cyanate ester resin prepolymer, polyphenylene ether, biphenyl type epoxy resin and methyl ethyl ketone is 1:1:1:0.4.

[0095] In the embodiment of the present invention, the specific preparation method of the modified spherical filler is as follows:

[0096] (1). Melt the glass raw materials, then perform water quenching and drying;

[0097] (2). Crush and grind the dried glass raw materials to obtain glass particles with a certain particle size;

[0098] (3). Then put the glass particles into the spheroidizing furnace for reheating, so that the molten glass particles are spheroidized under the action of surface tension;

[0099] (4). Then quickly cool and collect to obtain the modified spherical filler.

[0100] In the embodiment of the present invention, the glass raw materials in step (1) include components with the following mass ratios: 72% of silicon oxide, 19% of boron oxide, 4.5% of sodium oxide, 2.5% of potassium oxide, 1% of barium oxide, and 1% of others.

[0101] In the embodiment of the present invention, the specific treatment method of the modified reinforcing material is as follows:

[0102] 1), Bake the NE fiberglass cloth at a temperature of 40 °C for 30 minutes, and then naturally cool it to room temperature;

[0103] 2), Then immerse the heat-treated NE fiberglass cloth in the treatment liquid for 10 minutes and air-dry it naturally for 340 minutes;

[0104] 3), Then place it in a drying oven at 100 °C and dry it for 2 hours.

[0105] A manufacturing method of a high-frequency and high-speed copper clad laminate, characterized in that it specifically includes the following steps:

[0106] S1, Take raw materials in proportion and set aside;

[0107] S2, Put the modified resin and the accelerator into a high-shear reactor and stir for 8 hours;

[0108] S3, Then add the modified spherical filler while stirring, and then stir at high speed for 4 hours to obtain glue;

[0109] S4, Coat the surface of the modified reinforcing material with the glue prepared in step S3, and then bake it in a drying oven for 10 minutes to make a prepreg;

[0110] S5, Cut the prepreg obtained in step S4, then stack the cut prepregs neatly together. After reaching an appropriate stacking height, cover copper foils on its upper and lower surfaces, and then put it into a vacuum hot press for hot pressing and forming.

[0111] In the embodiment of the present invention, the thickness of the copper foil in step S5 is 9 μm.

[0112] In the embodiment of the present invention, the temperature in the vacuum hot press in step S5 is 230 °C, the pressure is 450 N, and the pressing time is 4 hours.

[0113] Combined with the above technical solutions, the present invention can reduce the curing reaction temperature of the system by adding polyphenylene ether to the bisphenol A cyanate ester resin prepolymer / biphenyl type epoxy resin system. This is mainly because polyphenylene ether has the characteristic of catalyzing the reaction of the bisphenol A cyanate ester resin prepolymer, which can accelerate the curing reaction of the bisphenol A cyanate ester resin prepolymer. By using silicon oxide and boron oxide as the basic components of the low-dielectric spherical filler, and introducing sodium oxide and potassium oxide at the same time, the acid and alkali resistance of the glass is improved, and the glass melting temperature is reduced by introducing barium oxide. The spheroidization effect is obvious, and the sphericity can generally reach more than 0.950, with good fluidity. During subsequent use, the resin dosage can be greatly reduced. Even under the premise of high addition amount, the resin viscosity will not increase significantly, improving the production operation conditions and significantly increasing the production efficiency.

[0114] Meanwhile, the content not detailedly described in this specification belongs to the prior art well-known to those skilled in the art.

[0115] It should be noted that, in this article, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or sequence between these entities or operations. Moreover, the term "comprising", "including" or any other variation thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article or device.

[0116] Although the embodiments of the present invention have been shown and described, it will be understood by those of ordinary skill in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention. The scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-frequency and high-speed copper clad laminate, comprising a copper clad laminate body, characterized in that, The copper clad laminate body is made by steps of batching, curing, cutting, pre-laminating combination and hot pressing forming, and the materials used include modified resin, modified spherical filler, modified reinforcing material and accelerator, and are proportioned by the following weight parts: 50-60 parts of modified resin, 8-15 parts of modified spherical filler, 8-14 parts of modified reinforcing material and 5-15 parts of accelerator.

2. The high-frequency and high-speed copper clad laminate according to claim 1, wherein: The specific preparation method of the modified resin is as follows: First, weigh a certain amount of bisphenol A cyanate ester resin prepolymer and polyphenylene ether and blend them, then add an appropriate amount of methyl ethyl ketone to dissolve them. After they are completely dissolved, add a certain weight ratio of biphenyl type epoxy resin.

3. The high-frequency and high-speed copper clad laminate according to claim 2, wherein: The weight ratio of the bisphenol A cyanate ester resin prepolymer, polyphenylene ether, biphenyl type epoxy resin and methyl ethyl ketone is 1:1:1:0.

4.

4. A high-frequency and high-speed copper clad laminate according to claim 1, characterized in that: The specific preparation method of the modified spherical filler is as follows: (1). Melt the glass raw materials, then perform water quenching and drying. (2). Crush and grind the dried glass raw materials to obtain glass particles with a certain particle size. (3). Then put the glass particles into the spheroidizing furnace for reheating, so that the molten glass particles are spheroidized under the action of surface tension. (4). Then quickly cool and collect to obtain the modified spherical filler.

5. The high-frequency and high-speed copper clad laminate according to claim 4, wherein: The glass raw materials in the step (1) include the following components by mass ratio: 72% of silicon oxide, 19% of boron oxide, 4.5% of sodium oxide, 2.5% of potassium oxide, 1% of barium oxide and 1% of others.

6. The high-frequency and high-speed copper clad laminate according to claim 1, characterized in that: The specific treatment method of the modified reinforcing material is as follows: 1). Bake the NE glass fiber cloth at a temperature of 40 °C for 30 minutes, and then naturally cool it to room temperature. 2). Then immerse the heat-treated NE glass fiber cloth in the treatment liquid for 10-18 minutes and air dry it naturally for 30-40 minutes. 3). Then place it in a drying oven at 100 °C and dry it for 2 hours.

7. A manufacturing method of a high-frequency and high-speed copper clad laminate according to any one of claims 1-6, characterized in that, Specifically, it includes the following steps: S1. Take raw materials in proportion and set aside. S2. Put the modified resin and accelerator into a high-shear reaction kettle and stir for 5-8 hours. S3. Then add the modified spherical filler while stirring, and then stir at high speed for 2-4 hours to obtain glue. S4. Coat the surface of the modified reinforcing material with the glue prepared in step S3, and then bake it in a drying oven for 8-10 minutes to make a semi-cured sheet. S5. Cut the semi-cured sheet obtained in step S4, then stack the cut semi-cured sheets neatly together. After reaching an appropriate stacking height, cover copper foils on its upper and lower surfaces, and then put it into a vacuum hot press for hot pressing forming.

8. The manufacturing method of the high-frequency and high-speed copper clad laminate according to claim 7, characterized in that: The thickness of the copper foil in the step S5 is 9 μm.

9. The manufacturing method of the high-frequency and high-speed copper clad laminate according to claim 7, characterized in that: The temperature in the vacuum hot press in the step S5 is 135-230 °C, the pressure is 80-450 N, and the pressing time is 4 hours.

Citation Information

Patent Citations

  • High-frequency and high-speed copper clad laminate manufacturing method and its copper clad laminate

    CN107234851B