Comprehensive utilization device and method for limonite type laterite-nickel ore based on fluidized selective reduction

Through the integration of fluidization selective reduction technology and multi-stage process, the problem of low utilization rate of nickel-cobalt iron in limon-type laterite nickel ore is solved, and efficient step-by-step recycling and cascade utilization of nickel-cobalt iron is achieved, energy consumption and waste slag emissions are reduced, and high-value lithium battery materials and steel raw materials are produced.

CN120485511APending Publication Date: 2025-08-15NORTHEASTERN UNIV CHINA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510769587.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-10
Publication Date
2025-08-15

AI Technical Summary

Technical Problem

Among the existing treatment methods for limonite-type laterite nickel ore, the comprehensive utilization rate of nickel-cobalt iron is low, the iron resources are seriously wasted, and the high-pressure acid leaching process has problems such as equipment corrosion, high energy consumption, and large leaching slag emissions.

Method used

The fluidized selective reduction technology is adopted, and through multi-stage process integration, including preheating, fluidized reduction, atmospheric acid leaching, phosphate precipitation and other steps, the step-by-step enrichment and cascade utilization of nickel-cobalt iron are achieved, combined with waste gas heat recovery, and the resource recovery process is optimized.

Benefits of technology

It improves the comprehensive recycling efficiency of nickel-cobalt iron, reduces waste slag emissions, realizes the recycling of iron resources, improves resource utilization, reduces energy consumption and production costs, and produces high-value products that are in line with lithium battery materials and steel raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120485511A_ABST
    Figure CN120485511A_ABST
Patent Text Reader

Abstract

The invention discloses a comprehensive utilization device and method for limonite type laterite-nickel ore based on fluidization selective reduction, and belongs to the technical field of mineral processing and metallurgy. Through system integration and targeted optimization of a multi-stage process, preheating drying and selective reduction are completed when a material is in a fluidized state; meanwhile, heat energy recycling is achieved through a waste gas heat recycling device, enrichment and extraction of metal nickel and cobalt and graded recycling and utilization of associated iron resources are achieved through subsequent normal-pressure acid leaching, phosphate precipitation reaction and stage magnetic separation, and products can meet the utilization requirements of lithium battery materials and steel raw materials. According to the method, the resource recovery efficiency and the process coherence are effectively improved, and efficient step-by-step recovery and gradient utilization of nickel, cobalt, iron and other multi-metal resources in the limonite type laterite-nickel ore are synergistically achieved through process integration and function segmentation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of mineral processing and metallurgy, and in particular relates to a device and method for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction. Background Art

[0002] Nickel is a key strategic metal, widely used in stainless steel manufacturing, battery materials, electroplating, catalysts, and other fields. As the most important metal in battery manufacturing, nickel also plays a key role in energy storage. With the rapid development of new energy vehicles and the energy storage industry, global demand for metals such as nickel and cobalt continues to increase. The gradual depletion of nickel sulfide ore resources has prompted people to turn their attention to laterite nickel ore, which has more abundant reserves.

[0003] In recent years, the proportion of laterite nickel ore used in smelting has reached as high as 70%. Limonitic laterite nickel ore, a polymetallic resource containing nickel, cobalt, and iron, is characterized by high Fe and Co contents and low Ni content. Its primary phases are goethite and hematite, with gangue components primarily consisting of spinel, talc, and amphibole. Nickel is primarily present in the goethite via lattice substitution or adsorption. High-pressure acid leaching (HPAL) is currently the mainstream process for processing limonitic laterite nickel ore, which has high iron content and low silicon and magnesium content. It boasts high nickel and cobalt leaching rates (>90%) and is widely used by companies such as MCC Ramu New Energy, GEM Co., Ltd., Ningbo Liqin Mining Company, BHP Billiton (Australia), CVRD (CNV), and Falconbridge (Canada). However, this process requires high magnesium (<5%) and aluminum content in the ore. These factors can easily precipitate and form scale, leading to severe corrosion in equipment and impacting productivity. At the same time, the amount of leached residue discharged is large and cannot be recycled, resulting in a significant waste of iron resources. Furthermore, high energy consumption and equipment costs, large amounts of sulfuric acid, and demanding control of reaction temperature and pressure significantly increase production costs. Therefore, achieving the comprehensive utilization of valuable components such as nickel, cobalt, and iron in limonitic laterite nickel ore is of great significance.

[0004] Patent CN117646119A discloses a method for processing laterite nickel ore. The method involves recovering nickel and cobalt through a process of beneficiation, high-pressure acid leaching, circulating leaching, slurry neutralization, CCD washing, underflow filter press, and reduction smelting, with the by-product being ferrosilicon. This method, based on existing conventional methods for extracting nickel and cobalt, reduces and smelts the leaching residue from high-pressure acid leaching of laterite nickel ore to produce ferrosilicon. This method not only addresses the environmental concerns associated with the production of large amounts of leaching residue, but also achieves the commercialization and high value-added of iron and silicon. However, the high sulfur content in the leaching residue can easily lead to excessive sulfur content in the ferrosilicon obtained from the reduction smelting process, affecting product quality. Furthermore, the reduction smelting process requires high temperatures of 1400°C to 1700°C, and requires a large amount of reducing agent, blue coke or coke (80% to 100% of the leaching residue mass), resulting in high energy consumption and production costs, making it difficult to implement industrially. Patent CN106987728A discloses a method for leaching nickel and cobalt from laterite nickel ore using atmospheric pressure phosphoric acid and simultaneously preparing iron phosphate. First, the limonitic laterite nickel ore is subjected to a roasting and transformation treatment at 300°C to 400°C before leaching. Subsequently, phosphoric acid is used as a leaching agent and an atmospheric pressure acid leaching process is adopted to leach the roasted and transformed laterite nickel ore. After solid-liquid separation, nickel and cobalt enter the solution, and iron is enriched in the leaching residue in the form of iron phosphate, thereby achieving selective leaching, separation and comprehensive utilization of nickel, cobalt and iron. However, the obtained iron phosphate product contains high levels of impurities such as SiO2, Al2O3, and Cr2O3, which will affect the quality of the iron phosphate product. Further purification treatment is required before it can be used as a raw material for manufacturing lithium iron phosphate batteries, catalysts, ceramics, etc.

[0005] Therefore, there is an urgent need to develop a comprehensive utilization device and method for limonitic laterite nickel ore based on fluidized selective reduction, which can not only improve the comprehensive recovery efficiency of nickel, cobalt and iron, but also effectively reduce waste slag emissions and realize the recycling of iron resources, which has important practical significance. Summary of the Invention

[0006] In response to the problems of low comprehensive resource utilization rate, waste of iron resources and tailings storage in the development process of the above-mentioned existing limonitic laterite nickel ore, the present invention provides a limonitic laterite nickel ore comprehensive utilization device and method based on fluidized selective reduction. Through the system integration and targeted optimization of multi-stage processes, it overcomes the limitations of the existing technology that only focuses on single metal recovery or single process optimization, realizes organic synergy between various process units, effectively improves resource recovery efficiency and process connectivity, and further realizes the step-by-step recovery and cascade efficient utilization of multi-metal resources such as nickel, cobalt, and iron in limonitic laterite nickel ore, providing a feasible new path for green metallurgy and resource recycling.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] A comprehensive utilization device for limonitic laterite nickel ore based on fluidized selective reduction, comprising: a feeding system, a preheating system, a fluidized reduction system, a leaching system, a product synthesis preparation system, a magnetic separation system, and a dust removal system;

[0009] Among them, the feeding system includes a silo and screw feeder I and screw feeder II;

[0010] The preheating system includes a primary cyclone preheater, a secondary cyclone preheater, a fluidized roasting main furnace, a burner and a primary cyclone separator;

[0011] The fluidized reduction system includes a fluidized reduction reactor and a secondary cyclone separator;

[0012] The leaching system includes a water quenching pulping tank and a leaching reaction tank;

[0013] The product synthesis preparation system includes a synthesis reactor, a drying device, a filtering device, a nickel-cobalt solution storage device and a ferric phosphate dihydrate collection device;

[0014] The magnetic separation system includes a first magnetic separator, a mill, a second magnetic separator, a magnetic concentrate recovery device and a tailings recovery device;

[0015] The dust removal system includes a cyclone dust collector, a bag dust collector, and a Roots blower.

[0016] The bottom of the silo is connected to the screw feeder I and the feed port of the first-stage cyclone preheater in sequence; the bottom discharge port of the first-stage cyclone preheater is connected to the feed port of the second-stage cyclone preheater through a pipeline, and the top air outlet of the first-stage cyclone preheater is connected to the air inlet of the cyclone dust collector through a pipeline; the bottom discharge port of the second-stage cyclone preheater is connected to the lower feed port of the fluidized roasting main furnace through a pipeline; a combustion station is provided at the bottom of the fluidized roasting main furnace, and the top of the fluidized roasting main furnace is connected to the first-stage cyclone separator through a pipeline, and the exhaust gas outlet of the first-stage cyclone separator is connected to the feed port of the second-stage cyclone preheater;

[0017] The bottom discharge port of the first-stage cyclone separator is connected to the top feed port of the fluidized reduction reactor, the screw feeder II is connected to the top feed port of the fluidized reduction reactor through a pipeline, the upper discharge port of the fluidized reduction reactor is connected to the feed port of the second-stage cyclone separator, the top air outlet of the second-stage cyclone separator is connected to the air inlet of the fluidized roasting main furnace through a pipeline, and the bottom discharge port of the second-stage cyclone separator is connected to the water quenching pulping tank through a pipeline;

[0018] The bottom of the water quenching pulping tank is connected to the leaching reaction tank; the liquid outlet of the leaching reaction tank is connected to the liquid inlet of the synthesis reactor; the liquid outlet of the synthesis reactor is connected to the filtering device, the solid discharge port of the filtering device is connected to the drying device and the ferric phosphate dihydrate collecting device in sequence through a pipeline, and the liquid outlet of the filtering device is connected to the nickel-cobalt solution storage device.

[0019] The solid material discharge port of the leaching reaction tank, the mill, the first magnetic separator and the second magnetic separator are connected in sequence through pipelines; the magnetic concentrate discharge port and the tailings discharge port of the second magnetic separator are connected to the magnetic concentrate recovery device and the tailings recovery device respectively.

[0020] The air outlet of the cyclone dust collector is connected to the air inlet of the bag dust collector through a pipeline, and the bottom discharge port of the cyclone dust collector and the bottom discharge port of the bag dust collector are connected to the feed port of the screw feeder II through a pipeline; the air outlet of the bag dust collector is connected to the air inlet of the Roots blower.

[0021] A gas distribution plate is provided at the bottom of the fluidized roasting main furnace; a partition is provided inside the fluidized reduction reactor to divide the fluidized reduction reactor into a feed chamber and a reaction chamber, and a gas distribution plate is provided at the bottom; a gap is left between the lower part of the partition and the gas distribution plate provided at the bottom of the reactor as a material flow channel; a feed port is provided at the top of the feed chamber, which is connected to the discharge port of the first-stage cyclone separator; a discharge port is provided on the side wall of the reaction chamber, which is connected to the inlet of the second-stage cyclone separator; and the reducing gas outlet of the fluidized reduction reactor is connected to a burner;

[0022] A stirring device is provided in the water quenching pulp making tank;

[0023] The magnetic separator is a wet drum magnetic separation device.

[0024] Based on the same inventive concept, the present invention also provides a method for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction, which is implemented using the above-mentioned device and comprises the following steps:

[0025] Step 1: placing limonitic laterite nickel ore powder with a particle size of ≤1.0 mm and a water content of ≤10% in a silo, starting a screw feeder I, and evenly conveying the material to a primary cyclone preheater at a set flow rate; wherein the portion with a particle size less than 0.074 mm accounts for 45% to 60% of the total mass; the chemical composition of the limonitic laterite nickel ore is, by mass percentage, as follows: Ni 0.5% to 1.3%, TFe 40% to 50%, Co 0.1% to 0.3%, SiO2 3% to 5%, Al2O3 4% to 6%, CaO 4% to 6%, and MgO 0.5% to 5%.

[0026] Step 2: The material is preheated in the first-stage cyclone preheater. The ratio of the gas volume flow rate to the mass flow rate of the solid material being processed in the system is 0.10m 3 / kg~0.30m 3 / kg, the preheated solid material enters the secondary cyclone preheater; the dust particles discharged from the primary cyclone preheater and the dust particles collected by the cyclone dust collector and bag dust collector are recovered together to the fluidized reduction reactor, and the exhaust gas is discharged to the outside of the system through the Roots blower;

[0027] Step 3: The solid material is further heated to 400°C to 650°C in the secondary cyclone preheater; the preheated solid material after gas-solid separation enters the fluidized roasting main furnace, forms a fluidized state under the action of negative pressure and high-temperature flue gas, and is further heated and dried at 750°C to 900°C. The dried material is separated into gas and solid in the primary cyclone separator, and the separated gas returns to the secondary cyclone preheater for preheating; the temperature of the high-temperature flue gas is 600°C to 800°C;

[0028] Step 4: The preheated material obtained by the primary cyclone separator is fed into a fluidized reduction reactor, where a reduction reaction occurs in a reducing gas environment to obtain a reduced material; the reaction temperature is 500° C. to 600° C., and the reaction time is 10 min to 30 min; the reducing gas is obtained by mixing H2 and CO produced by coal gasification or natural gas cracking with N2 in proportion; the sum of the volume concentrations of H2 and CO is controlled to be 25% to 45%, wherein the volume concentration of H2 is 15% to 30%, and the volume concentration of CO is 10% to 15%;

[0029] Step 5: The reduced material is separated by a secondary cyclone separator, and the unreacted excess reducing gas is recovered to the fluidized bed roasting main furnace for combustion and heat supply. The solid product enters the water quenching pulp making tank for atmospheric pressure acid leaching. After the acid leaching is completed, solid-liquid separation is performed to obtain leachate and leaching residue. The slurry is heated to 60°C to 90°C using the waste heat of the reduced material. The slurry is discharged into the leaching reaction tank for atmospheric pressure acid leaching, with a sulfuric acid concentration of 0.5M to 1.5M, an acid leaching temperature of 60°C to 90°C, an acid leaching time of 20min to 60min, a stirring speed of 200rpm to 600rpm, and a pH value controlled below 2.

[0030] Step 6: After the leached slag is ground to -0.074mm, accounting for 80% to 90%, it is fed into the first magnetic separator for magnetic roughing with a magnetic field strength of 150kA / m to 200kA / m. The roughing concentrate and roughing tailings obtained from the roughing are fed into the second magnetic separator for cleaning with a magnetic field strength of 80kA / m to 150kA / m to obtain iron concentrate with a total iron (TFe) grade of ≥56% and cleaned tailings. The roughing tailings and cleaned tailings are combined as raw materials for cement production.

[0031] Step 7: placing the leachate in a synthesis reactor, first adding 1 / 3 of the oxidant for pre-oxidation treatment, and then sequentially adding a regulator, a phosphate precipitant and the remaining oxidant to react; the reaction product is subjected to solid-liquid separation, and the filter residue is dried to obtain battery-grade ferric phosphate dihydrate, and the filtrate is used for the subsequent production of nickel cobalt sulfate or nickel cobalt hydroxide products; the phosphate precipitant is at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate or phosphoric acid; the oxidant is hydrogen peroxide; the molar ratio of the total amount of the oxidant added to the divalent iron ions in the leachate is 0.5 to 1.0; and the molar ratio of phosphate ions to iron ions is 1.0 to 1.05.

[0032] The present invention uses multi-stage fluidized drying and dehydration, and then uses a fluidized selective reduction process to accurately control the reduction reaction conditions, so that the iron oxides in the limonite are selectively converted into a strongly magnetic magnetite phase; at the same time, the nickel oxide and cobalt oxide in the lattice are reduced to metallic nickel and cobalt that are easily acid-soluble (metallization rate ≥ 95%); unlike the acid leaching process in the prior art that is simply used for nickel and cobalt leaching, the selective reduction of the present invention is combined with a normal pressure sulfuric acid leaching collaborative process to achieve step-by-step enrichment of nickel, cobalt and iron. Metallic nickel and cobalt are preferentially selectively dissolved into the leachate, while the generated magnetite is relatively acid-resistant and remains in the leach residue. After solid-liquid separation, nickel-cobalt leachate and iron-rich leach residue are obtained, thereby realizing the extraction and recovery of nickel and cobalt in limonite-type laterite nickel ore; the nickel-cobalt leachate is prepared by adding hydrogen peroxide oxidant and phosphate precipitant, and controlling the pH value of the solution to make the Fe in the leachate 2+ Oxidation to form Fe 3+ And finally precipitate out in the form of ferric phosphate dihydrate, thereby co-producing battery-grade ferric phosphate products and realizing the high-value utilization of iron in nickel-cobalt leachate. Compared with the single leaching process in the prior art, this process realizes the simultaneous advancement of nickel-cobalt separation and iron resource utilization. A grinding-two-stage magnetic separation multi-stage process is adopted for iron-rich leaching slag to improve the dissociation degree of iron minerals and enhance the magnetic separation effect. The iron concentrate obtained by magnetic separation can be used as a standardized raw material for ironmaking, while the magnetic separation tailings are used as auxiliary raw materials in cement production, thereby constructing a tailing-free process, realizing comprehensive recovery and efficient utilization of resources, and effectively improving resource utilization. The present invention is based on a device and method for fluidized selective reduction and step-by-step recovery and cascade utilization of multi-metal resources, which has the characteristics of simple process, efficient and clean, high-value utilization, etc., and improves the comprehensive utilization efficiency of limonitic laterite nickel ore resources, providing a feasible new path for green metallurgy and resource recycling.

[0033] The basic principle of the present invention is to use multi-stage cyclone preheating and fluidized roasting main furnace to heat the solid material to the required reaction temperature. After heating, the material enters the fluidized reduction reactor in its own heat storage state, contacts with the reducing gas and rapidly undergoes a reduction reaction, thereby reducing the target elements such as nickel, cobalt, and iron to soluble active metals Ni and Co, and insoluble and highly magnetic Fe3O4 (magnetite). This process effectively eliminates the effects of colloidal minerals such as limonite on Ni. 2+ and Co 2 + The adsorption of ions significantly increases the subsequent atmospheric sulfuric acid leaching rate of nickel and cobalt. Leaching residue can be converted into iron concentrate through selective grinding and magnetic separation, achieving comprehensive iron resource recovery. Furthermore, magnetic separation tailings can be used as a high-quality raw material for cement production. A phosphate precipitant is introduced into the nickel-cobalt leachate to precipitate the iron ions in the leachate into battery-grade iron phosphate, achieving high-value utilization of the iron ions in the leachate.

[0034] Compared with the existing methods for processing and utilizing limonitic laterite nickel ore, the device and method proposed in the present invention achieve the efficient extraction and resource utilization of multiple components such as nickel, cobalt, and iron through process integration and functional segmentation. The present invention can simultaneously obtain nickel-cobalt leaching solution, battery-grade iron phosphate, qualified iron concentrate, and magnetic tailings that can be used as raw materials for cement production, achieving full component separation and tailing-free disposal of ore, and breaking through the technical difficulties of tailings storage and iron resource waste in traditional high-pressure acid leaching processes. Preheating, drying, and selective reduction are completed when the material is in a fluidized state, effectively improving the gas-solid mass transfer and heat transfer efficiency, achieving precise control of the mineral phase transformation during the process, and at the same time combining with the waste gas heat recovery device to achieve heat energy recycling and reduce the system roasting energy consumption; subsequently, through normal pressure acid leaching, phosphate precipitation reaction, and staged magnetic separation, the enrichment and extraction of metal nickel and cobalt and the graded recovery of associated iron resources are achieved, and the output can meet the utilization needs of lithium battery materials and steel raw materials. The overall process route realizes the efficient, clean and tailing-free disposal of low-grade nickel oxide ore, and provides a new solution for the fractional utilization and green metallurgy of complex laterite nickel ore resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of a device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to the present invention;

[0036] In the figure, 1. silo, 2. screw feeder I, 3. primary cyclone preheater, 4. secondary cyclone preheater, 5. fluidized bed roasting main furnace, 6. primary cyclone separator, 7. fluidized bed reduction reactor, 8. secondary cyclone separator, 9. burner, 10. water quenching pulping tank, 11. cyclone dust collector, 12. bag dust collector, 13. screw feeder II, 14. Roots blower, 15. leaching reaction tank, 16. synthesis reactor, 17. grinding mill, 18. first magnetic separator, 19. second magnetic separator, 20. magnetic concentrate recovery device, 21. nickel-cobalt solution storage device, 22. drying device, 23. ferric phosphate dihydrate collection device, 24. filtering device, 25. tailings recovery device. DETAILED DESCRIPTION

[0037] The technical solution of the present invention will be further described below with reference to the accompanying drawings and through specific embodiments. Those skilled in the art should understand that the embodiments are only for the purpose of helping to understand the present invention and should not be regarded as specific limitations of the present invention.

[0038] The present invention provides a comprehensive utilization device for limonitic laterite nickel ore based on fluidized selective reduction, comprising: a feeding system, a preheating system, a fluidized reduction system, a leaching system, a product synthesis and preparation system, a magnetic separation system and a dust removal system; wherein the feeding system comprises a silo and screw feeder I and screw feeder II; the preheating system comprises a primary cyclone preheater, a secondary cyclone preheater, a fluidized roasting main furnace, a burner and a primary cyclone separator; the fluidized reduction system comprises a fluidized reduction reactor and a secondary cyclone separator; the leaching system comprises a water quenching pulping tank and a leaching reaction tank; the product synthesis and preparation system comprises a synthesis reactor, a drying device, a nickel-cobalt solution storage device and a ferric phosphate dihydrate collecting device; the magnetic separation system comprises a mill, a first magnetic separator, a second magnetic separator, a magnetic concentrate recovery device and a tailings recovery device; and the dust removal system comprises a cyclone dust collector, a bag dust collector and a Roots blower.

[0039] In the device provided by the present invention, each component has the following functions:

[0040] The silo is used to store limonitic laterite nickel ore powder. The bottom of the silo is connected to the feed port of the first-stage cyclone preheater through a screw feeder I.

[0041] The screw feeder I is used to convey the material in the silo to the first-stage cyclone preheater at a set flow rate. The feed port is connected to the bottom of the silo, and the discharge port is connected to the feed port of the first-stage cyclone preheater.

[0042] The first-stage cyclone preheater is used to preheat the laterite nickel ore powder and perform gas-solid separation. The discharge port is connected to the feed port of the second-stage cyclone preheater, and the exhaust gas outlet is connected to the cyclone dust collector.

[0043] The cyclone dust collector is used to capture dust particles discharged from the first-stage cyclone preheater. The discharge port is transported to the fluidized reduction reactor through the screw feeder I, and the exhaust gas outlet is connected to the bag dust collector.

[0044] The bag filter is used to further remove fine dust particles from the exhaust gas. The exhaust gas is discharged to the outside of the system through a Roots blower.

[0045] The Roots blower is used to discharge the exhaust gas from the bag dust collector out of the system while maintaining a negative pressure state to prevent dust leakage.

[0046] The secondary cyclone preheater is used to further heat the solid material discharged from the primary cyclone preheater. The discharge port is connected to the feed port of the fluidized bed roasting main furnace, and the exhaust gas outlet is connected to the inlet of the primary cyclone preheater to achieve heat recovery.

[0047] The bottom of the fluidized roasting main furnace is equipped with a burner that generates high-temperature flue gas by burning natural gas or coal-based gas. This high-temperature flue gas enters the main furnace through the bottom gas distribution plate, fluidizing the material. The top of the main furnace is connected to the first cyclone separator via a pipe. The exhaust gas outlet is connected to the inlet of the second-stage cyclone preheater, and the flue gas is returned for preheating.

[0048] The primary cyclone separator is used to separate the material and flue gas discharged from the fluidized bed roasting main furnace. The material outlet is connected to the feed inlet of the fluidized bed reduction reactor, and the flue gas outlet is connected to the inlet of the secondary cyclone preheater for flue gas recycling.

[0049] The fluidized reduction reactor is equipped with a partition that divides the reactor into a feed chamber and a reaction chamber. A gas distribution plate is located at the bottom, allowing nitrogen and reducing gas to flow in. A gap is left between the lower portion of the partition and the gas distribution plate at the bottom of the reactor, providing a flow channel for the materials. A feed inlet is located at the top of the feed chamber, connecting to the discharge port of the first cyclone separator. A discharge port is located on the sidewall of the reaction chamber, connecting to the inlet of the second cyclone separator for transporting the reduced material after the reaction. The reducing gas outlet is connected to a burner, enabling the recycling of unreacted gases.

[0050] The secondary cyclone separator is used to separate the gas-solid mixture discharged from the fluidized reduction reactor. The material outlet is connected to the feed inlet of the water quenching pulping tank, and the gas outlet is connected to the burner to achieve gas recovery circulation.

[0051] The water quenching pulping tank includes a cooling tank and a stirring device, which heats the pulp by the waste heat in the reducing material. The discharge port is connected to the feed port of the leaching reaction tank.

[0052] The leaching tank is equipped with a stirring device for atmospheric pressure acid leaching of the reduced ore pulp. The discharge port is connected to the mill feed port, which in turn is connected to the feed port of the first magnetic separator. The first magnetic separator's discharge port is connected to the feed port of the second magnetic separator, which is used to further concentrate the iron ore. The concentrate outlet of the first magnetic separator is connected to the concentrate outlet of the second magnetic separator.

[0053] The first and second magnetic separators: wet drum magnetic separation equipment.

[0054] The synthesis reactor is used to add an oxidant and a phosphate precipitant to the nickel-cobalt leaching solution to carry out the iron phosphate precipitation reaction. The discharge port is connected to the inlet of the filtration device.

[0055] The present invention provides a method for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction, which is implemented using the above-mentioned device and comprises the following steps:

[0056] Step 1: placing limonitic laterite nickel ore powder with a particle size of ≤1.0 mm and a water content of ≤10% in a silo, wherein the portion with a particle size less than 0.074 mm accounts for 45% to 60% of the total mass; the chemical composition of the limonitic laterite nickel ore is as follows, by mass percentage: Ni 0.5% to 1.3%, TFe 40% to 50%, Co 0.1% to 0.3%, SiO2 3% to 5%, Al2O3 4% to 6%, CaO 4% to 6%, and MgO 0.5% to 5%; starting screw feeder I to uniformly convey the material to the first-stage cyclone preheater at a set flow rate;

[0057] Step 2: The material is preheated in the first-stage cyclone preheater. The ratio of the gas volume flow rate to the mass flow rate of the solid material being processed in the system is 0.10m 3 / kg~0.30m 3 / kg, the preheated solid material enters the secondary cyclone preheater; the dust particles discharged from the primary cyclone preheater and the dust particles collected by the cyclone dust collector and bag dust collector are recovered together to the fluidized reduction reactor, and the exhaust gas is discharged to the outside of the system through the Roots blower;

[0058] Step 3: The solid material is further heated to 400°C to 650°C in the secondary cyclone preheater; the preheated solid material after gas-solid separation enters the fluidized roasting main furnace, where it is fluidized under negative pressure and high-temperature flue gas (600°C to 800°C); the material is further heated and dried at 750°C to 900°C, and the dried material is separated into gas and solid in the primary cyclone separator, and the separated gas returns to the secondary cyclone preheater for preheating;

[0059] Step 4: The preheated material obtained from the primary cyclone separator is fed into a fluidized reduction reactor. The reaction temperature of the material in the reactor is 500° C. to 600° C., and the reaction time is 10 min to 30 min. The reducing gas used is a mixture of hydrogen (H2), carbon monoxide (CO), and nitrogen (N2) produced by coal gasification or natural gas cracking. The sum of the volume concentrations of H2 and carbon monoxide is controlled to be 25% to 45%, wherein the volume concentration of H2 is 15% to 30%, and the volume concentration of CO is 10% to 15%.

[0060] The key chemical reactions occurring within the reactor include:

[0061] 3Fe2O3+CO / H2=2Fe3O4+CO2 / H2O (1)

[0062] CoO+CO / H2=Co+CO2 / H2O (2)

[0063] NiO+CO / H2=Ni+CO2 / H2O (3)

[0064] Step 5: The reduced material is separated by a secondary cyclone separator, and the unreacted excess reducing gas is recycled to the fluidized bed roasting main furnace for combustion and heat supply; the solid product enters the water quenching pulping pool, and the waste heat of the reduced material is used to heat the slurry to 60℃~90℃. The slurry is discharged into the leaching reaction tank for atmospheric pressure acid leaching, with a sulfuric acid concentration of 0.5M~1.5M, an acid leaching temperature of 60℃~90℃, an acid leaching time of 20min~60min, a stirring speed of 200rpm~600rpm, and a pH value controlled below 2. After the acid leaching is completed, solid-liquid separation is carried out to obtain leachate and leach residue;

[0065] Step 6: After the leached slag is ground to -0.074mm, accounting for 80% to 90%, it is fed into the first magnetic separator for magnetic roughing with a magnetic field strength of 150kA / m to 200kA / m. After magnetic separation, pre-selected coarse concentrate and tailings are obtained. The pre-selected coarse concentrate is fed into the second magnetic separator for fine separation with a magnetic field strength of 80kA / m to 150kA / m to obtain qualified iron concentrate with a total iron (TFe) grade of ≥56% and magnetic tailings. The tailings from the two magnetic separations are combined and used as raw materials for cement production.

[0066] Step 7: Place the leachate in a synthesis reactor, first add 1 / 3 of the oxidant for pre-oxidation treatment, then add the regulator (sulfuric acid, sodium hydroxide), phosphate precipitant (at least one of diammonium phosphate, diammonium hydrogen phosphate, ammonium phosphate or phosphoric acid) and the remaining oxidant (the molar ratio of the oxidant to divalent iron ions is 0.5 to 1.0, and the preferred oxidant is hydrogen peroxide), and the molar ratio of phosphate ions to iron ions is 1.0 to 1.05. React at 15°C to 25°C, pH = 1.5 to 2.0, for 30min to 60min, with a stirring speed of 150rpm to 300rpm, and then keep warm for 60min to 120min to promote the precipitation of iron phosphate. The main equations of the oxidation reaction and precipitation reaction are:

[0067] 2Fe 2+ +H2O2+2H + =2Fe 3+ +2H2O (4)

[0068] 2H2O+Fe 3+ +PO4 3- =FePO4·2H2O↓ (5)

[0069] The reaction product is separated into solid and liquid, and the filter residue is dried at 105°C to obtain battery-grade ferric phosphate dihydrate. The filtrate is used for the subsequent production of nickel cobalt sulfate or nickel cobalt hydroxide products.

[0070] The reduction reactor of the present invention is provided with a partition inside, which divides the reactor into a feed chamber and a reaction chamber. A gas distribution plate is provided at the bottom. There is a gap between the lower part of the partition and the gas distribution plate at the bottom of the reactor as a material flow channel. A feed port is provided at the top of the feed chamber, and a discharge port is provided on the side wall of the reaction chamber.

[0071] To further describe the present invention, the device and method of the present invention are further described in detail below with reference to the accompanying drawings and embodiments.

[0072] Example 1:

[0073] The embodiment of the present invention provides a comprehensive utilization device for limonitic laterite nickel ore based on fluidized selective reduction, such as Figure 1 As shown, it includes a feeding system, a preheating system, a fluidized reduction system, a leaching system, a product synthesis preparation system, a magnetic separation system and a dust removal system.

[0074] The feeding system includes a silo 1 and screw feeder I2 and screw feeder II 13; the preheating system includes a primary cyclone preheater 3, a secondary cyclone preheater 4, a fluidized roasting main furnace 5, a burner 9 and a primary cyclone separator 6; the fluidized reduction system includes a fluidized reduction reactor 7 and a secondary cyclone separator 8; the leaching system includes a water quenching pulping pool 10 and a leaching reaction tank 15; the product synthesis preparation system includes a synthesis reactor 16, a drying device 22, a filtering device 24, a nickel-cobalt solution storage device 21 and a dihydrate iron phosphate collection device 23; the magnetic separation system includes a mill 17, a first magnetic separator 18, a second magnetic separator 19, a magnetic concentrate recovery device 20 and a tailings recovery device 25; the dust removal system includes a cyclone dust collector 11, a bag dust collector 12 and a Roots blower 14.

[0075] The bottom of the silo 1 is connected to the screw feeder Ⅰ2 and the feed port of the first-level cyclone preheater 3 in sequence; the bottom discharge port of the first-level cyclone preheater 3 is connected to the feed port of the second-level cyclone preheater 4 through a pipeline, and the top air outlet of the first-level cyclone preheater 3 is connected to the air inlet of the cyclone dust collector 11 through a pipeline; the bottom discharge port of the second-level cyclone preheater 4 is connected to the lower feed port of the fluidized roasting main furnace 5 through a pipeline; a combustion station is provided at the bottom of the fluidized roasting main furnace 5, and the top of the fluidized roasting main furnace 5 is connected to the first-level cyclone separator 6 through a pipeline, and the exhaust gas outlet of the first-level cyclone separator 6 is connected to the feed port of the second-level cyclone preheater 4;

[0076] The bottom discharge port of the first-stage cyclone separator 6 is connected to the top feed port of the fluidized reduction reactor 7, the screw feeder II 13 is connected to the top feed port of the fluidized reduction reactor 7 through a pipeline, the upper discharge port of the fluidized reduction reactor 7 is connected to the feed port of the second-stage cyclone separator 8, the top air outlet of the second-stage cyclone separator 8 is connected to the air inlet of the fluidized roasting main furnace 5 through a pipeline, and the bottom discharge port of the second-stage cyclone separator 8 is connected to the water quenching pulping tank 10 through a pipeline; the bottom of the water quenching pulping tank 10 is connected to the leaching reaction tank 15; the liquid outlet of the leaching reaction tank 15 is connected to the liquid inlet of the synthesis reactor 16; the liquid outlet of the synthesis reactor 16 is connected to the filtering device 24, the solid discharge port of the filtering device 24 is connected to the drying device 22 and the dihydrate iron phosphate collecting device 23 in sequence through a pipeline, and the liquid outlet of the filtering device 24 is connected to the nickel-cobalt solution storage device 21.

[0077] The solid material discharge port of the leaching reaction tank 15, the mill 17, the first magnetic separator 18, and the second magnetic separator 19 are connected in sequence through pipelines; the magnetic concentrate discharge port and the tailings discharge port of the second magnetic separator 19 are connected to the magnetic concentrate recovery device 20 and the tailings recovery device 25 respectively.

[0078] The air outlet of the cyclone dust collector 11 is connected to the air inlet of the bag dust collector 12 through a pipeline, and the bottom discharge port of the cyclone dust collector 11 and the bottom discharge port of the bag dust collector 12 are connected to the feed port of the screw feeder II 13 through a pipeline; the air outlet of the bag dust collector 12 is connected to the air inlet of the Roots blower 14.

[0079] A gas distribution plate is provided at the bottom of the fluidized roasting main furnace 5; a partition is provided inside the fluidized reduction reactor 7, which divides the fluidized reduction reactor 7 into a feed chamber and a reaction chamber, and a gas distribution plate is provided at the bottom; a gap is left between the lower part of the partition and the gas distribution plate provided at the bottom of the reactor as a material flow channel; a feed port is provided at the top of the feed chamber, which is connected to the discharge port of the first-stage cyclone separator 6; a discharge port is provided on the side wall of the reaction chamber, which is connected to the inlet of the second-stage cyclone separator 8; the reducing gas outlet of the second-stage cyclone separator 8 is connected to the burner 9 at the bottom of the fluidized roasting main furnace;

[0080] The water quenching pulping tank 10 includes a stirring device;

[0081] The first magnetic separator 18 is a wet drum magnetic separator. Limonitic laterite nickel ore is placed in a silo 1. The ore has a Ni grade of 0.76%, a Co grade of 0.22%, and contains, by weight, 42.82% TFe, 4.59% SiO2, 5.07% Al2O3, 5.45% CaO, and 1.86% MgO. The solids have a particle size of ≤1 mm, with particles smaller than 0.074 mm accounting for 55% of the total mass. The ore contains 9.12% water by mass.

[0082] Start the Roots blower 14 to form negative pressure in the bag dust collector 12, cyclone dust collector 11, first-stage cyclone preheater 3, second-stage cyclone preheater 4, fluidized bed roasting main furnace 5, and first-stage separation cyclone 6; the ratio of the gas volume flow rate of the cyclone preheating system to the mass flow rate of the mixed material is 0.15m 3 / k;

[0083] Turn on the burner 9, introduce natural gas and air into the burner 9, and feed high-temperature flue gas into the bottom of the fluidized bed roasting main furnace 5 through the burner 9. Under the action of negative pressure, the high-temperature flue gas passes through the first-stage separation cyclone 6, the second-stage cyclone preheater 4, the first-stage cyclone preheater 3, the cyclone dust collector 11, the bag dust collector 12 and the Roots blower 14 in sequence;

[0084] The screw feeder I2 is started to feed the laterite nickel ore powder in the silo 1 into the primary cyclone preheater 3 to obtain the primary preheated material, which is then fed into the secondary cyclone preheater 4 to be preheated to 450°C to obtain the secondary preheated material, and then enters the fluidized roasting main furnace 5 through the feed port at the bottom of the fluidized roasting main furnace 5;

[0085] Under the action of high-temperature flue gas and negative pressure, the secondary preheated material is fluidized in the fluidized roasting main furnace 5 and further heated to 750°C. The heated material is then discharged from the discharge pipe at the top of the fluidized roasting main furnace 5 along with the airflow into the primary cyclone separator 6. After gas-solid separation, the heated material enters the reduction reactor under the action of gravity.

[0086] After the first stage preheating, the gas-solid separation of the first stage exhaust gas passes through the cyclone dust collector 11 and the bag dust collector 12 in sequence to obtain dust material and exhaust gas. The exhaust gas is sucked into the atmosphere by the Roots blower 14, and the dust material is fed into the fluidized reduction reactor 7 through the screw feeder II 13;

[0087] Nitrogen and reducing gas are introduced into the nitrogen inlet and reducing gas inlet of the fluidized reduction reactor 7, respectively. Under the action of nitrogen and reducing gas, the solid material is in a state of intense fluidized motion and undergoes a reduction reaction with the reducing gas in the fluidized reduction reactor 7. The temperature of the solid material during the reduction reaction in the fluidized reduction reactor 7 is 520° C. The total volume concentration of H2 and CO in the reducing gas entering the fluidized reduction reactor 7 is 45%, of which the volume concentration of H2 is 30% and the volume concentration of CO is 15%. The ratio of the volume flow rate of the reducing gas entering the fluidized reduction reactor 7 to the mass flow rate of the solid material is 0.10m 3 / kg, the reaction time is 20 min, and the reduced material formed flows out from the discharge port of the fluidized reduction reactor 7 along with the air flow;

[0088] The reduced material flowing out of the discharge port of the fluidized reduction reactor 7 enters the secondary cyclone separator 8. The secondary solid material after gas-solid separation is fed into the water quenching pulping tank 10. The excess reduced gas after separation enters the burner of the burner 9 and is burned as fuel in the fluidized roasting main furnace 5.

[0089] The secondary solid material is water-quenched and cooled in a water-quenching pulping tank 10. The waste heat carried by the solid material controls the pulp temperature to 80°C. The solid material is then fed into a leaching reaction tank 15 and mixed with a 15% sulfuric acid solution for acid leaching. The liquid-solid ratio is 3:1, the leaching temperature is 80°C, the leaching time is 40 minutes, and the process pH value is 1.5-1.7. After solid-liquid separation, leaching residue and leachate are obtained. The leaching residue is fed into a mill 17 and ground to a content of -0.074mm accounting for 80%. The leaching residue is then subjected to a roughing separation and a concentrating separation in a first magnetic separator 18 and a second magnetic separator 19 under magnetic separator field strengths of 150kA / m and 80kA / m, respectively, to obtain a magnetic concentrate with a TFe grade of 56.43% and a recovery rate of 81.30%.

[0090] The nickel-cobalt leachate was added with 1 / 3 hydrogen peroxide and stirred, and then diammonium hydrogen phosphate solution, the remaining hydrogen peroxide, and the adjusting agent were added to the synthesis reactor 16 for synthesis reaction. During the process, the iron-phosphorus (Fe / P) molar ratio of the feed was maintained at 1, the reaction temperature was 25°C, the stirring speed was 240 rpm, the stirring time was 60 min, and the pH value during the stirring process was 1.7-2. After the synthesis, the material was kept warm in the reactor for 60 min and then filtered to obtain a nickel-cobalt filtrate and a filter residue. The filter residue of the iron phosphate product was dried at 105°C to obtain dihydrated iron phosphate. The various indicators of the dihydrated iron phosphate product are shown in Table 1. The prepared dihydrated iron phosphate product meets the HG / T 4701-2021 battery grade standard.

[0091] Table 1 Analysis of various indicators of battery-grade ferric phosphate dihydrate products

[0092]

[0093] Example 2:

[0094] The limonitic laterite nickel ore has a Ni grade of 1.28% and a Co grade of 0.18%. It contains 49.83% TFe, 3.22% SiO2, 4.08% Al2O3, 4.10% CaO, and 0.71% MgO by mass. The particle size of the solid part is ≤1.2mm, of which the part with a particle size less than 0.074mm accounts for 45% of the total mass. It contains 9.36% water by mass.

[0095] The method is the same as Example 1, except that:

[0096] (1) The temperature of the material after preheating in the first-stage cyclone preheater 3 and the second-stage cyclone preheater 4 is 550°C;

[0097] (2) The preheated material is further heated to 800° C. in the fluidized bed roasting main furnace 5;

[0098] (3) The temperature of the material during the reduction reaction in the fluidized reduction reactor 7 is 600° C., and the reduction time is 15 min. The total volume concentration of H2 and CO in the reducing gas entering the fluidized reduction reactor 7 is 25%, of which the volume concentration of H2 is 15% and the volume concentration of CO is 10%. The ratio of the volume flow rate of the reducing gas entering the fluidized reduction reactor 7 to the mass flow rate of the solid material is 0.25 m 3 / kg;

[0099] (4) The solid material was mixed with a 12% sulfuric acid solution for acid leaching reaction, with a liquid-to-solid ratio of 3:1, a temperature of 80°C, a leaching time of 30 minutes, and a pH value of 1.8-2;

[0100] (5) The leached residue was ground in mill 17 until the content of -0.074 mm accounted for 90%, and then the leached residue was subjected to a roughing and a concentrating process in a magnetic separator at field strengths of 200 kA / m and 150 kA / m, respectively, to obtain a magnetic concentrate with a TFe grade of 56.60% and a recovery rate of 70.06%.

[0101] (6) The ferric phosphate synthesis reaction in the leachate was carried out with a molar ratio of iron to phosphorus (Fe / P) of 1, a reaction temperature of 24°C, a stirring speed of 260 rpm, a stirring time of 30 min, and a process pH value of 1.7 to 1.8. The synthesized material was kept warm in the synthesis reactor 16 for 60 min, then filtered and dried at 105°C to obtain ferric phosphate dihydrate. The product indicators of ferric phosphate dihydrate were TFe: 30.12%, P: 17.02%, iron-phosphorus ratio (Fe / P): 0.980, particle size (D50): 4.64 μm, and tap density: 0.64 g / cm 3 , Moisture: 19.94% meets battery grade standards.

[0102] Example 3:

[0103] The limonitic laterite nickel ore has a Ni grade of 1.17% and a Co grade of 0.25%. It contains 46.89% TFe, 3.88% SiO2, 5.02% Al2O3, 4.89% CaO, and 1.25% MgO by mass. The particle size of the solid part is ≤1.5mm, of which the part with a particle size of less than 0.074mm accounts for 48% of the total mass. It contains 8.99% water by mass.

[0104] The method is the same as Example 1, except that:

[0105] (1) The temperature of the material after preheating in the first-stage cyclone preheater 3 and the second-stage cyclone preheater 4 is 500°C;

[0106] (2) The preheated material is further heated to 820° C. in the fluidized bed roasting main furnace 5;

[0107] (3) The temperature of the material during the reduction reaction in the fluidized reduction reactor 7 is 580° C., and the reduction time is 16 min. The total volume concentration of H2 and CO in the reducing gas entering the fluidized reduction reactor 7 is 35%, of which the volume concentration of H2 is 20% and the volume concentration of CO is 15%. The ratio of the volume flow rate of the reducing gas entering the fluidized reduction reactor 7 to the mass flow rate of the solid material is 0.30 m 3 / kg;

[0108] (4) The solid material was mixed with a 10% sulfuric acid solution for acid leaching at a liquid-to-solid ratio of 3:1, a temperature of 90°C, a leaching time of 55 min, and a pH value of 1.6 to 1.8;

[0109] (5) The leached residue was ground in mill 17 until the content of -0.074 mm accounted for 85%, and then the leached residue was subjected to a roughing and a concentrating process in a magnetic separator at field strengths of 180 kA / m and 100 kA / m, respectively, to obtain a magnetic concentrate with a TFe grade of 56.40% and a recovery rate of 69.93%;

[0110] (6) The ferric phosphate synthesis reaction in the leachate was carried out with a molar ratio of iron to phosphorus (Fe / P) of 1, a reaction temperature of 20°C, a stirring speed of 240 rpm, a stirring time of 60 min, and a process pH value of 1.9 to 2.0. The synthesized material was kept warm in the synthesis reactor 16 for 90 min, then filtered and dried at 105°C to obtain ferric phosphate dihydrate. The product indicators of ferric phosphate dihydrate were TFe: 29.89%, P: 16.77%, iron-phosphorus ratio (Fe / P): 0.988, particle size (D50): 3.92 μm, and tap density: 0.72 g / cm 3 , Moisture: 20.12% meets battery grade standards.

[0111] Example 4:

[0112] The limonitic laterite nickel ore has a Ni grade of 0.86% and a Co grade of 0.17%. It contains 42.69% TFe, 4.52% SiO2, 5.59% Al2O3, 5.40% CaO, and 3.85% MgO by mass. The particle size of the solid part is ≤1.5mm, of which the part with a particle size of less than 0.074mm accounts for 50% of the total mass. It contains 9.87% water by mass.

[0113] The method is the same as Example 1, except that:

[0114] (1) The temperature of the material after preheating in the first-stage cyclone preheater 3 and the second-stage cyclone preheater 4 is 600°C;

[0115] (2) The preheated material is further heated to 850° C. in the fluidized bed roasting main furnace 5;

[0116] (3) The temperature of the material during the reduction reaction in the fluidized reduction reactor 7 is 550° C., and the reduction time is 18 min. The total volume concentration of H2 and CO in the reducing gas entering the fluidized reduction reactor 7 is 40%, of which the volume concentration of H2 is 25% and the volume concentration of CO is 15%. The ratio of the volume flow rate of the reducing gas entering the fluidized reduction reactor 7 to the mass flow rate of the solid material is 0.18 m 3 / kg;

[0117] (4) The solid material was mixed with a 15% sulfuric acid solution for acid leaching, with a liquid-to-solid ratio of 3:1, a temperature of 60°C, a leaching time of 50 min, and a process pH value of 1.7-2;

[0118] (5) The leached residue was ground in mill 17 to a content of -0.074 mm, accounting for 88%. Subsequently, the leached residue was subjected to a roughing and a concentrating process in a magnetic separator under field intensities of 170 kA / m and 120 kA / m, respectively, to obtain a magnetic concentrate with a TFe grade of 55.23% and a recovery rate of 75.86%.

[0119] (6) The ferric phosphate synthesis reaction in the leachate was carried out with a molar ratio of iron to phosphorus (Fe / P) of 1, a reaction temperature of 25°C, a stirring speed of 240 rpm, a stirring time of 45 min, and a process pH value of 1.7 to 1.8. The synthesized material was kept warm in the synthesis reactor 16 for 180 min, then filtered, and dried at 105°C to obtain ferric phosphate dihydrate. The product indicators of ferric phosphate dihydrate were TFe: 30.01%, P: 16.87%, iron-phosphorus ratio (Fe / P): 0.987, particle size (D50): 5.12 μm, and tap density: 0.69 g / cm 3 , Moisture: 19.82% meets battery grade standards.

[0120] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.

Claims

1. A comprehensive utilization device for limonitic laterite nickel ore based on fluidized selective reduction, characterized in that: include: Feeding system, preheating system, fluidized reduction system, leaching system, product synthesis preparation system, magnetic separation system and dust removal system.

2. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 1, characterized in that: The feeding system includes a silo and screw feeder I and screw feeder II; The preheating system includes a primary cyclone preheater, a secondary cyclone preheater, a fluidized roasting main furnace, a burner and a primary cyclone separator; The fluidized reduction system includes a fluidized reduction reactor and a secondary cyclone separator; The leaching system includes a water quenching pulping tank and a leaching reaction tank; The product synthesis preparation system includes a synthesis reactor, a drying device, a filtering device, a nickel-cobalt solution storage device and a ferric phosphate dihydrate collection device; The magnetic separation system includes a first magnetic separator, a mill, a second magnetic separator, a magnetic concentrate recovery device and a tailings recovery device; The dust removal system includes a cyclone dust collector, a bag dust collector, and a Roots blower.

3. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 2, characterized in that: The bottom of the silo is connected to the screw feeder I and the first-level cyclone preheater feed port in sequence; the bottom discharge port of the first-level cyclone preheater is connected to the second-level cyclone preheater feed port through a pipeline, and the top air outlet of the first-level cyclone preheater is connected to the air inlet of the cyclone dust collector through a pipeline; the bottom discharge port of the second-level cyclone preheater is connected to the lower feed port of the fluidized roasting main furnace through a pipeline; a combustion station is provided at the bottom of the fluidized roasting main furnace, the top of the fluidized roasting main furnace is connected to the first-level cyclone separator through a pipeline, and the exhaust gas outlet of the first-level cyclone separator is connected to the second-level cyclone preheater feed port.

4. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 2, characterized in that: The bottom discharge port of the first-stage cyclone separator is connected to the top feed port of the fluidized reduction reactor, the screw feeder II is connected to the top feed port of the fluidized reduction reactor through a pipeline, the upper discharge port of the fluidized reduction reactor is connected to the feed port of the second-stage cyclone separator, the top air outlet of the second-stage cyclone separator is connected to the air inlet of the fluidized roasting main furnace through a pipeline, and the bottom discharge port of the second-stage cyclone separator is connected to the water quenching pulping tank through a pipeline; wherein, a stirring device is provided in the water quenching pulping tank.

5. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 2, characterized in that: The bottom of the water quenching pulping tank is connected to the leaching reaction tank; the liquid outlet of the leaching reaction tank is connected to the liquid inlet of the synthesis reactor; the liquid outlet of the synthesis reactor is connected to the filtering device, the solid discharge port of the filtering device is connected to the drying device and the ferric phosphate dihydrate collecting device in sequence through a pipeline, and the liquid outlet of the filtering device is connected to the nickel-cobalt solution storage device.

6. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 2, characterized in that: The solid material discharge port of the leaching reaction tank, the mill, the first magnetic separator and the second magnetic separator are connected in sequence through pipelines; the magnetic concentrate discharge port and the tailings discharge port of the second magnetic separator are connected to the magnetic concentrate recovery device and the tailings recovery device respectively.

7. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 2, characterized in that: The air outlet of the cyclone dust collector is connected to the air inlet of the bag dust collector through a pipeline, and the bottom discharge port of the cyclone dust collector and the bottom discharge port of the bag dust collector are connected to the feed port of the screw feeder II through a pipeline; the air outlet of the bag dust collector is connected to the air inlet of the Roots blower.

8. The device for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 2, characterized in that: A gas distribution plate is provided at the bottom of the fluidized roasting main furnace; a partition is provided inside the fluidized reduction reactor to divide the fluidized reduction reactor into a feed chamber and a reaction chamber, and a gas distribution plate is provided at the bottom; a gap is left between the lower part of the partition and the gas distribution plate provided at the bottom of the reactor, serving as a material flow channel; a feed port is provided at the top of the feed chamber, which is connected to the discharge port of the first-stage cyclone separator; a discharge port is provided on the side wall of the reaction chamber, which is connected to the inlet of the second-stage cyclone separator; and the reducing gas outlet of the fluidized reduction reactor is connected to the burner.

9. A method for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction, which is implemented by the method according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Place limonitic laterite nickel ore powder with a particle size of ≤1.0 mm and a moisture content of ≤10% in a silo, start screw feeder I, and evenly convey the material to the first-stage cyclone preheater at a set flow rate; the portion with a particle size of less than 0.074 mm accounts for 45% to 60% of the total mass; Step 2: The material is preheated in the first-stage cyclone preheater. The ratio of the gas volume flow rate to the mass flow rate of the solid material being processed in the system is 0.10m 3 / kg~0.30m 3 / kg, the preheated solid material enters the secondary cyclone preheater; the dust particles discharged from the primary cyclone preheater and the dust particles collected by the cyclone dust collector and bag dust collector are recovered together to the fluidized reduction reactor, and the exhaust gas is discharged to the outside of the system through the Roots blower; Step 3: The solid material is further heated to 400°C to 650°C in the secondary cyclone preheater; the preheated solid material after gas-solid separation enters the fluidized roasting main furnace, forms a fluidized state under the action of negative pressure and high-temperature flue gas, and is further heated and dried at 750°C to 900°C. The dried material is separated into gas and solid in the primary cyclone separator, and the separated gas returns to the secondary cyclone preheater for preheating; the temperature of the high-temperature flue gas is 600°C to 800°C; Step 4: The preheated material obtained from the primary cyclone separator is fed into a fluidized reduction reactor, where a reduction reaction occurs under a reducing gas environment to obtain a reduced material; Step 5: The reduced material is separated by a secondary cyclone separator, and the unreacted excess reducing gas is recovered to the fluidized bed roasting main furnace for combustion and heat supply. The solid product enters the water quenching slurry tank for atmospheric pressure acid leaching. After the acid leaching is completed, solid-liquid separation is performed to obtain leachate and leach residue. Step 6: After the leached residue is ground to -0.074mm, accounting for 80% to 90%, it is fed into the first magnetic separator for magnetic roughing to obtain roughing concentrate and roughing tailings; the pre-selected roughing concentrate is fed into the second magnetic separator for cleaning to obtain iron concentrate with a total iron (TFe) grade of ≥56% and cleaned tailings. The roughing tailings and cleaned tailings are combined as raw materials for cement production; Step 7: The leachate is placed in a synthesis reactor, and 1 / 3 of the oxidant is first added for pre-oxidation treatment, followed by the addition of a regulator, a phosphate precipitant, and the remaining oxidant for reaction; the reaction product is subjected to solid-liquid separation, and the filter residue is dried to obtain battery-grade ferric phosphate dihydrate, and the filtrate is used for the subsequent production of nickel cobalt sulfate or nickel cobalt hydroxide products.

10. The method for comprehensive utilization of limonitic laterite nickel ore based on fluidized selective reduction according to claim 9, characterized in that: The slurry is discharged into the leaching reaction tank for atmospheric pressure acid leaching, the sulfuric acid concentration is 0.5M~1.5M, the acid leaching temperature is 60℃~90℃, the acid leaching time is 20min~60min, the stirring speed is 200rpm~600rpm, and the pH value is controlled below 2; In step 7, the adjusting agent is sulfuric acid or sodium hydroxide; the phosphate precipitant is at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate or phosphoric acid; the oxidant is hydrogen peroxide; the molar ratio of the total amount of the oxidant added to the divalent iron ions in the leachate is 0.5 to 1.0; and the molar ratio of phosphate ions to iron ions is 1.0 to 1.05.

Citation Information

Patent Citations

  • Method for normal-pressure phosphoric-acid leaching of nickel-cobalt and synchronous preparation of iron phosphate

    CN106987728A