A textile with good moisture absorption and quick-drying properties
By using a double-layer composite structure and modified polyester fiber design, combined with nano-magnesium oxide and antibacterial agents, the shortcomings of textiles in terms of moisture absorption, quick drying and antibacterial properties are solved, achieving rapid moisture absorption, rapid drying and highly effective antibacterial effects.
Patent Information
- Application Number
- CN202510754370.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-06-06
AI Technical Summary
Existing textiles have shortcomings in terms of moisture absorption and quick-drying properties and antibacterial properties. In particular, they are prone to bacterial growth in humid environments, which affects wearing comfort and makes it difficult to maintain excellent performance over a long period of time.
It adopts a double-layer composite structure, with modified polyester fiber and cotton fiber blended together. The inner loop layer contains high cotton fiber moisture absorption, while the outer antibacterial base fabric layer conducts moisture through a microporous structure. Nano magnesium oxide and antibacterial agents are added to the polyester fiber to form a gradient moisture absorption and conduction path, which improves the moisture absorption, quick drying and antibacterial ability of the textile.
It achieves rapid moisture absorption, rapid drying, and highly effective antibacterial properties in textiles, with a moisture absorption rate of over 8.5%, an evaporation rate of 0.27-0.31 g/h.cm2, and an antibacterial rate of over 99%, significantly improving wearing comfort and health safety.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of textile manufacturing technology, specifically to a textile with good moisture absorption and quick-drying properties. Background Technology
[0002] In the textile industry, moisture-wicking and quick-drying performance is one of the important indicators for evaluating the comfort of functional fabrics. Currently, most moisture-wicking and quick-drying textiles on the market use single fibers or simple blended structures, such as pure cotton or polyester-cotton blends. Although cotton fibers can quickly absorb sweat due to their hydrophilicity, their drying speed is relatively slow, which can easily cause the wearer to feel damp and uncomfortable; while polyester fibers have good quick-drying properties, their moisture absorption is poor, making it difficult to meet high moisture absorption requirements.
[0003] Furthermore, traditional textiles also have shortcomings in antibacterial properties, especially in humid environments where bacteria can easily grow, affecting not only wearing comfort but also potentially causing health problems. Current technologies attempt to improve antibacterial properties by adding antibacterial agents or using finishing processes, but these methods often suffer from poor durability, short-lasting antibacterial effects, or negative impacts on fiber properties. Therefore, developing a textile that combines excellent moisture-wicking and quick-drying properties with antibacterial capabilities has become a pressing challenge in the current technological field. Summary of the Invention
[0004] This invention proposes a textile with good moisture absorption and quick-drying properties, which solves the defects in related technologies.
[0005] The technical solution of the present invention is as follows: The preparation process of a textile with good moisture absorption and quick-drying properties is as follows: Step 1: Blend modified polyester fiber with cotton fiber, then immerse in a 10% sodium hypochlorite solution, adjust the pH to neutral, and soak for 10-20 minutes to obtain an antibacterial base fabric layer; the antibacterial base fabric layer contains 60%-65% by weight of modified polyester fiber and the remainder of cotton fiber. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 20%-30% by weight of polyester fibers and the remainder of cotton fibers; Step 3: Combine the antibacterial base fabric layer with the terry cloth layer to obtain the finished product.
[0006] In a more optimized manner, the preparation process of the modified polyester fiber is as follows: A1: Mix nano-magnesium oxide, polyester, and antibacterial agent to obtain a premix; A2: Feed the premixed material into a twin-screw extruder, melt-blend at 260-280℃, cool and granulate to obtain antibacterial masterbatch; A3: The antibacterial masterbatch is mixed with polyester, heated and melted, then extruded through a spinneret, cooled and solidified, and stretched and shaped to obtain modified polyester fiber.
[0007] More preferably, the premix comprises the following components: by weight, 2-3 parts of nano magnesium oxide, 0.5-1 parts of antibacterial agent, and 95-100 parts of polyester.
[0008] Ideally, the mass ratio of the antibacterial masterbatch to polyester is 1:8-9.
[0009] In a more optimized manner, the preparation process of the antibacterial agent is as follows: S1: Dissolve 5,5-dimethylhydantoin and potassium hydroxide in anhydrous ethanol, raise the temperature to 85°C, reflux and stir for 10-15 min, then slowly add 1-bromo-3-chloropropane, continue to reflux at 85°C for 8-10 h, and then perform post-treatment to obtain intermediate A. S2: Mix intermediate A, 6-dimethylamino-1-hexanol and ethanol, raise the temperature to 60-70℃, reflux for 10-12 h, after the reaction is completed, slowly add the reaction solution dropwise to tetrahydrofuran, filter, and obtain intermediate B; S3: Mix intermediate B, glycerol triglycidyl ether, and ethanol, add boron trifluoride diethyl ether complex, raise the temperature to 60-70℃, reflux for 1-2 hours, after the reaction is complete, cool to room temperature, add saturated sodium bicarbonate solution to quench the reaction, adjust the pH to neutral, filter, wash, and dry to obtain the antibacterial agent.
[0010] In this scheme, potassium hydroxide deprotonates the nitrogen atom of 5,5-dimethylhydantoin to generate a nitrogen anion intermediate with strong nucleophilicity. This intermediate then acts as a nucleophile to attack the α-carbon atom of 1-bromo-3-chloropropane, yielding intermediate A. The specific reaction process is shown below:
[0011] More preferably, intermediate A comprises the following raw materials: 14-16 parts by weight of 5,5-dimethylhydantoin, 6-8 parts by weight of potassium hydroxide, 60-80 parts by weight of anhydrous ethanol, and 17-18 parts by weight of 1-bromo-3-chloropropane.
[0012] In the process, 6-dimethylamino-1-hexanol undergoes a nucleophilic substitution reaction with the terminal chlorine atom of intermediate A to give intermediate B. The specific reaction process is shown below:
[0013] More preferably, intermediate B comprises the following raw materials: 21-23 parts by weight of intermediate A, 12-13 parts by weight of 6-dimethylamino-1-hexanol, and 50-60 parts by weight of ethanol.
[0014] In the scheme, boron trifluoride diethyl ether complex, as a Lewis acid, complexes with the epoxy oxygen atom of glycerol triglycidyl ether, making the epoxy carbon atom positively charged, and reacts with the hydroxyl group contained in intermediate B to obtain the antibacterial agent.
[0015] More preferably, the antibacterial agent comprises the following raw materials: by weight, 30-32 parts intermediate B, 24-26 parts glycerol triglycidyl ether, 40-60 parts ethanol, and 0.7-0.8 parts boron trifluoride ethyl ether complex.
[0016] The advantages of this invention compared to existing technologies are as follows: This invention, by employing a double-layer composite structure and modifying polyester fibers, effectively improves the moisture absorption, quick-drying properties, and antibacterial capabilities of textiles; specifically as follows: Firstly, the solution optimizes moisture absorption and quick-drying performance through a gradient moisture absorption and wicking path. Specifically, the inner terry cloth layer, which comes into contact with the skin, preferentially absorbs sweat due to its high cotton fiber content. The hydroxyl groups in the cotton fibers form hydrogen bonds with water molecules, thus fixing the moisture. The outer antibacterial base fabric layer, with its microporous structure, quickly receives the moisture conducted by the terry cloth layer and diffuses the moisture to the external environment through the gaps between the fibers. This forms a gradient transport path of "inner layer moisture absorption - outer layer moisture wicking," shortening the moisture retention time.
[0017] Secondly, in the modification process of polyester fibers, nano-magnesium oxide and antibacterial agents work together as antibacterial fillers. Because the antibacterial agent contains epoxy groups, it not only improves its compatibility with polyester fibers but also acts as a binder, enhancing the compatibility between nano-magnesium oxide and polyester fibers, thereby improving the antibacterial ability of the textile. Furthermore, the antibacterial agent itself is a quaternary ammonium salt, which can generate N-chlorine structures during the subsequent sodium hypochlorite treatment of the antibacterial base fabric layer, further strengthening the antibacterial properties of the textile. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0019] Example 1: The preparation process of a textile with good moisture absorption and quick-drying properties is as follows: Step 1: Blend modified polyester fibers with cotton fibers, then immerse the blended fabric in a 10% sodium hypochlorite solution, adjust the pH to neutral, and soak for 10 minutes to obtain an antibacterial base fabric layer; the modified polyester fiber weight percentage in the antibacterial base fabric layer is 60%, and the cotton fiber weight percentage is 40%. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 20% polyester fibers by weight and 80% cotton fibers by weight. Step 3: Composite the antibacterial base fabric layer with the terry cloth layer to obtain the finished product; The preparation process of modified polyester fiber is as follows: A1: Mix 2 parts of nano magnesium oxide, 0.5 parts of antibacterial agent, and 95 parts of polyester chips to obtain a premix; A2: The premixed material is fed into a twin-screw extruder, melt-blended at 260°C, cooled and granulated to obtain antibacterial masterbatch; A3: The antibacterial masterbatch is mixed with polyester, heated and melted, then extruded through a spinneret, cooled and solidified, and stretched to obtain modified polyester fiber; the mass ratio of antibacterial masterbatch to polyester is 1:8; The preparation process of the antibacterial agent is as follows: S1: Dissolve 14 parts of 5,5-dimethylhydantoin and 6 parts of potassium hydroxide in 60 parts of anhydrous ethanol, raise the temperature to 85°C, reflux and stir for 10 min, then slowly add 17 parts of 1-bromo-3-chloropropane, continue to reflux at 85°C for 8 h, and then perform post-processing to obtain intermediate A. S2: Mix 21 parts of intermediate A, 12 parts of 6-dimethylamino-1-hexanol and 50 parts of ethanol, raise the temperature to 60°C, reflux for 10 h, after the reaction is completed, slowly add the reaction solution dropwise to tetrahydrofuran, filter, and obtain intermediate B. S3: Mix 30 parts of intermediate B, 24 parts of glycerol triglycidyl ether, and 40 parts of ethanol, add 0.7 parts of boron trifluoride diethyl ether complex, raise the temperature to 60°C, reflux for 1 hour, after the reaction is complete, cool to room temperature, add saturated sodium bicarbonate solution to quench the reaction, adjust the pH to neutral, filter, wash, and dry to obtain the antibacterial agent.
[0020] Example 2: The preparation process of a textile with good moisture absorption and quick-drying properties is as follows: Step 1: Blend modified polyester fibers with cotton fibers, then immerse the blended fabric in a 10% sodium hypochlorite solution, adjust the pH to neutral, and soak for 20 minutes to obtain an antibacterial base fabric layer; the modified polyester fiber weight percentage in the antibacterial base fabric layer is 65%, and the cotton fiber weight percentage is 35%. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 30% polyester fibers by weight and 70% cotton fibers by weight. Step 3: Composite the antibacterial base fabric layer with the terry cloth layer to obtain the finished product; The preparation process of modified polyester fiber is as follows: A1: Mix 3 parts of nano magnesium oxide, 1 part of antibacterial agent, and 100 parts of polyester chips to obtain a premix; A2: The premixed material is fed into a twin-screw extruder, melt-blended at 280°C, cooled and granulated to obtain antibacterial masterbatch; A3: The antibacterial masterbatch is mixed with polyester, heated and melted, then extruded through a spinneret, cooled and solidified, and stretched to obtain modified polyester fiber; the mass ratio of antibacterial masterbatch to polyester is 1:9; The preparation process of the antibacterial agent is as follows: S1: Dissolve 16 parts of 5,5-dimethylhydantoin and 8 parts of potassium hydroxide in 80 parts of anhydrous ethanol, raise the temperature to 85°C, reflux and stir for 15 min, then slowly add 18 parts of 1-bromo-3-chloropropane, continue to reflux at 85°C for 10 h, and then perform post-processing to obtain intermediate A. S2: Mix 23 parts of intermediate A, 13 parts of 6-dimethylamino-1-hexanol and 60 parts of ethanol, raise the temperature to 70°C, reflux for 12 hours. After the reaction is complete, slowly add the reaction solution dropwise to tetrahydrofuran, filter, and obtain intermediate B. S3: Mix 32 parts of intermediate B, 26 parts of glycerol triglycidyl ether, and 60 parts of ethanol, add 0.8 parts of boron trifluoride diethyl ether complex, raise the temperature to 70°C, reflux for 2 hours, after the reaction is complete, cool to room temperature, add saturated sodium bicarbonate solution to quench the reaction, adjust the pH to neutral, filter, wash, and dry to obtain the antibacterial agent.
[0021] Example 3: The preparation process of a textile with good moisture absorption and quick-drying properties is as follows: Step 1: Blend modified polyester fibers with cotton fibers, then immerse the blended fabric in a 10% sodium hypochlorite solution, adjust the pH to neutral, and soak for 15 minutes to obtain an antibacterial base fabric layer; the modified polyester fiber weight percentage in the antibacterial base fabric layer is 62.5%, and the cotton fiber weight percentage is 37.5%. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 25% polyester fiber by weight and 75% cotton fiber by weight. Step 3: Composite the antibacterial base fabric layer with the terry cloth layer to obtain the finished product; The preparation process of modified polyester fiber is as follows: A1: Mix 2.5 parts of nano magnesium oxide, 0.75 parts of antibacterial agent, and 97.5 parts of polyester chips to obtain a premix; A2: The premixed material is fed into a twin-screw extruder, melt-blended at 270°C, cooled and granulated to obtain antibacterial masterbatch; A3: The antibacterial masterbatch is mixed with polyester, heated and melted, then extruded through a spinneret, cooled and solidified, and stretched to obtain modified polyester fiber; the mass ratio of antibacterial masterbatch to polyester is 1:8.5; The preparation process of the antibacterial agent is as follows: S1: Dissolve 15 parts of 5,5-dimethylhydantoin and 7 parts of potassium hydroxide in 70 parts of anhydrous ethanol, raise the temperature to 85°C, reflux and stir for 12.5 min, then slowly add 17.5 parts of 1-bromo-3-chloropropane, and continue to reflux at 85°C for 9 h. After post-processing, intermediate A is obtained. S2: Mix 22 parts of intermediate A, 12.5 parts of 6-dimethylamino-1-hexanol and 55 parts of ethanol, raise the temperature to 65°C, and reflux for 11 hours. After the reaction is complete, slowly add the reaction solution to tetrahydrofuran, filter, and obtain intermediate B. S3: Mix 31 parts of intermediate B, 25 parts of glycerol triglycidyl ether, and 50 parts of ethanol, add 0.75 parts of boron trifluoride diethyl ether complex, raise the temperature to 65°C, reflux for 1.5 h, after the reaction is complete, cool to room temperature, add saturated sodium bicarbonate solution to quench the reaction, adjust the pH to neutral, filter, wash, and dry to obtain the antibacterial agent.
[0022] Comparative Example 1: The polyester fibers in the antibacterial base fabric layer were not modified, and the rest was the same as in Example 3, as follows: Step 1: Blend polyester fiber and cotton fiber to obtain an antibacterial base fabric layer; the modified polyester fiber weight percentage in the antibacterial base fabric layer is 62.5%, and the cotton fiber weight percentage is 37.5%. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 25% polyester fiber by weight and 75% cotton fiber by weight. Step 3: Combine the antibacterial base fabric layer with the terry cloth layer to obtain the finished product.
[0023] Comparative Example 2: No antibacterial agent was added to the modified polyester fiber; all other aspects were the same as in Example 3, as detailed below: Step 1: Blend modified polyester fibers with cotton fibers to obtain an antibacterial base fabric layer; the modified polyester fiber weight percentage in the antibacterial base fabric layer is 62.5%, and the cotton fiber weight percentage is 37.5%. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 25% polyester fiber by weight and 75% cotton fiber by weight. Step 3: Composite the antibacterial base fabric layer with the terry cloth layer to obtain the finished product; The preparation process of modified polyester fiber is as follows: A1: Mix 2.5 parts of nano-magnesium oxide and 97.5 parts of polyester chips to obtain a premix; A2: The premixed material is fed into a twin-screw extruder, melt-blended at 270°C, cooled and granulated to obtain antibacterial masterbatch; A3: The antibacterial masterbatch is mixed with polyester, heated and melted, then extruded through a spinneret, cooled and solidified, and stretched to obtain modified polyester fiber; the mass ratio of antibacterial masterbatch to polyester is 1:8.5.
[0024] Testing and experimentation: (1) Weigh the textiles obtained in the examples and comparative examples, immerse them in distilled water for 1 minute, drain them for 30 seconds, weigh them again, and calculate the absorption rate; then suspend the wet sample in a standard environment (temperature 25°C, humidity 65%), weigh it at regular intervals, and calculate the evaporation rate. (2) The antibacterial rate of the textiles obtained in the examples and comparative examples was tested according to GB / T20944.3-2008 standard. The tested bacteria were Escherichia coli and Staphylococcus aureus. The data obtained are shown in Table 1 below: Table 1
[0025] Conclusion: This invention successfully prepared a textile with both excellent moisture absorption and quick-drying properties and antibacterial function through a double-layer composite structure design and modification of polyester fibers. Experimental data show that the textiles in Examples 1-3 all achieved a moisture absorption rate of over 8.5% and an evaporation rate of 0.27-0.31 g / h.cm 2 Within the specified range. Meanwhile, regarding antibacterial properties, the examples showed antibacterial rates exceeding 99% against both Escherichia coli and Staphylococcus aureus, while Comparative Example 1 showed only 15.4%-18.1% antibacterial rates, and Comparative Example 2 showed 75.4%-76.1%, fully verifying the synergistic effect of nano-magnesium oxide and antibacterial agents in the modified polyester fiber.
[0026] In summary, the gradient moisture absorption and wicking path design achieves efficient moisture management through "inner layer moisture absorption - outer layer moisture wicking," while the structural design of the antibacterial agent not only improves compatibility but also enhances the antibacterial durability of the fiber. Therefore, this invention provides an effective solution to the problem of traditional textiles' difficulty in simultaneously achieving moisture absorption and quick-drying performance and antibacterial function, and has good market application value.
[0027] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A textile with good moisture absorption and quick-drying properties, characterized in that: The manufacturing process of the textile is as follows: Step 1: Blend modified polyester fiber with cotton fiber, then immerse in a 10% sodium hypochlorite solution for 10-20 minutes, and then adjust the pH to neutral to obtain an antibacterial base fabric layer; the antibacterial base fabric layer contains 60%-65% by weight of modified polyester fiber and the remainder of cotton fiber. Step 2: Blend polyester fibers with cotton fibers to obtain a terry layer; the terry layer contains 20%-30% by weight of polyester fibers and the remainder of cotton fibers; Step 3: Composite the antibacterial base fabric layer with the terry loop layer to obtain the finished product; wherein the antibacterial base fabric layer is the outer layer and the terry loop layer is the inner layer; The preparation process of modified polyester fiber is as follows: A1: Mix nano-magnesium oxide, polyester, and antibacterial agent to obtain a premix; A2: Feed the premixed material into a twin-screw extruder, melt-blend at 260-280℃, cool and granulate to obtain antibacterial masterbatch; A3: Antibacterial masterbatch is mixed with polyester, heated and melted, then extruded through a spinneret, cooled and solidified, and stretched and shaped to obtain modified polyester fiber; The preparation process of the antibacterial agent is as follows: S1: Dissolve 5,5-dimethylhydantoin and potassium hydroxide in anhydrous ethanol, raise the temperature to 85°C, reflux and stir for 10-15 min, then slowly add 1-bromo-3-chloropropane, continue to reflux at 85°C for 8-10 h, and then perform post-treatment to obtain intermediate A. S2: Mix intermediate A, 6-dimethylamino-1-hexanol and ethanol, raise the temperature to 60-70℃, reflux for 10-12 h, after the reaction is completed, slowly add the reaction solution dropwise to tetrahydrofuran, filter, and obtain intermediate B; S3: Mix intermediate B, glycerol triglycidyl ether, and ethanol, add boron trifluoride diethyl ether complex, raise the temperature to 60-70℃, reflux for 1-2 hours, after the reaction is complete, cool to room temperature, add saturated sodium bicarbonate solution to quench the reaction, adjust the pH to neutral, filter, wash, and dry to obtain the antibacterial agent.
2. The textile with good moisture absorption and quick-drying properties according to claim 1, characterized in that: The premix comprises the following components: by weight, 2-3 parts nano magnesium oxide, 0.5-1 parts antibacterial agent, and 95-100 parts polyester.
3. The textile with good moisture absorption and quick-drying properties according to claim 1, characterized in that: The mass ratio of the antibacterial masterbatch to polyester is 1:(8-9).
4. A textile with good moisture absorption and quick-drying properties according to claim 1, characterized in that: The synthesis of intermediate A comprises the following raw materials: by weight, 14-16 parts of 5,5-dimethylhydantoin, 6-8 parts of potassium hydroxide, 60-80 parts of anhydrous ethanol, and 17-18 parts of 1-bromo-3-chloropropane.
5. A textile with good moisture absorption and quick-drying properties according to claim 1, characterized in that: The synthesis of intermediate B comprises the following raw materials: by weight, 21-23 parts of intermediate A, 12-13 parts of 6-dimethylamino-1-hexanol, and 50-60 parts of ethanol.
6. A textile with good moisture absorption and quick-drying properties according to claim 1, characterized in that: The antibacterial agent is synthesized from the following raw materials: by weight, 30-32 parts intermediate B, 24-26 parts glycerol triglycidyl ether, 40-60 parts ethanol, and 0.7-0.8 parts boron trifluoride diethyl ether complex.
Citation Information
Patent Citations
Unidirectional moisture conducting knitted fabric and related clothing items, manufacturing methods and manufacturing systems
US20230407536A1
Triglycidyl compounds and their use
US3925407A