Metallized film for high-voltage dry-type direct-current support capacitor
Through the three-inner string structure and the design of zinc-aluminum alloy material, the balance problem between high-voltage DC-supported capacitors in the workplace strength and volume is solved, and high-pass current density and small-voltage metallized film are achieved, which improves the long-term operation reliability of the capacitor.
Patent Information
- Application Number
- CN202511036182.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-26
- Publication Date
- 2025-08-29
AI Technical Summary
The metallized films of existing high-voltage DC support capacitors are difficult to balance between high workplace strength and small volume, resulting in insufficient long-term operation reliability. The existing multi-in-line structures have problems such as low square resistance and low workplace strength in high-voltage applications.
The metallized film design adopts a three-inner string structure. Through the superposition of the first and second layers of metallized films, the zinc-aluminum alloy material and the design of different active areas is used to form an equivalent three-inner string structure, which improves the workplace strength and optimizes the film thickness and square resistance value to meet the needs of high-voltage DC support capacitors.
The high-pass current density and small volume metallized film are achieved, which improves the workplace strength of the capacitor to 240V/μm, reduces the capacitor size, and improves the safety and reliability of long-term operation.
Smart Images

Figure CN120565290A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallized films, and in particular relates to a metallized film for high-voltage dry-type DC support capacitors. Background Art
[0002] DC link capacitors are key components in converters, primarily providing voltage stabilization and filtering. Currently, dry-type DC link capacitors are widely used in new energy, rail transit, and smart grid applications. These capacitors share the characteristics of a dry-type structure, high voltage, and large capacity.
[0003] The rated voltage of the DC link capacitor depends on the voltage of the IGBT device in the converter power module. Currently, IGBT device voltage levels are primarily 3300V and 4500V. In recent years, domestic and international research institutions and device manufacturers have conducted extensive research on high-voltage, high-power IGBT technology. Some manufacturers have achieved IGBT devices rated at 6000V / 2000A. Furthermore, commercial IGCT devices and IGBTs produced by domestic and international device manufacturers have reached 6500V / 3000A.
[0004] The rated voltage of the DC link capacitors for power modules with a device voltage rating of 3300V is 2.2-2.4kV. The rated voltage of the DC link capacitors for power modules with a device voltage rating of 4500V is 2.8-3.0kV. The rated voltage of the DC link capacitors for power modules with device voltage ratings of 6000V and 6500V is 3.8-4.0kV. The first two types of DC capacitors are widely used in converters for new energy, rail transit, and smart grids. Small-capacity 3.8-4.0kV DC capacitors are used in converters for rail transit. Currently, large-capacity 3.8-4.0kV dry-type DC capacitors are still in the research and development stage.
[0005] Currently, metallized film used in DC link capacitors with voltages from 2.2 to 4.0 kV all utilize a two-inner-series structure, with an operating field strength typically designed to be 233 to 240 V / μm. Due to film thickness, the thickness of the metallized film used in these DC link capacitors has certain limitations. For 2.2 kV DC link capacitors, a 4.5 μm thick, two-inner-series metallized film is typically used, with an operating field strength of 244.4 V / μm. For 2.4 kV DC link capacitors, a 5 μm thick, two-inner-series metallized film is typically used, with an operating field strength of 240 V / μm. For 2.8 kV DC link capacitors, a 6 μm thick, two-inner-series metallized film is typically used, with an operating field strength of 233.3 V / μm. For 3.0 kV DC link capacitors, a 6 μm thick, two-inner-series metallized film is typically used, with an operating field strength of 250 V / μm. DC support capacitors with a voltage level of 3.0kV usually use a metallized film with a two-inner-series structure and a thickness of 7μm, and its operating field strength is 214.28V / μm. DC support capacitors with a voltage level of 3.8kV usually use a metallized film with a two-inner-series structure and a thickness of 8μm, and its operating field strength is 237.5V / μm. DC support capacitors with a voltage level of 4kV usually use a metallized film with a two-inner-series structure and a thickness of 8μm, and its operating field strength is 250V / μm. DC support capacitors with a voltage level of 4kV usually use a metallized film with a two-inner-series structure and a thickness of 9μm, and its operating field strength is 222.2V / μm.
[0006] For 3 and 4 kV voltage-level capacitors, the operating field strength of DC link capacitors with corresponding metallized film thickness varies significantly, influenced by film thickness. Higher operating field strengths require smaller dimensions, but lower long-term reliability. Conversely, lower operating field strengths require larger dimensions, but higher long-term reliability.
[0007] Document CN 108597866 A discloses a metallized film with a multi-internal string structure. This technology is primarily targeted at metallized power capacitors, particularly metallized AC capacitors used for compensation in applications with higher voltages (AC2000V and above) or where voltage fluctuations are frequent or overcurrents are severe. The film is internally equivalent to multiple capacitors in series, eliminating the need to form conventional metallized film into individual film capacitor cores and then connect several of these cores in series to form a single capacitor. This technology not only saves costs and reduces processing steps, but also reduces product failure rates. However, the technology has the following drawbacks: The operating field strength of metallized AC capacitors is 50-60V / μm; the three-internal string structure in this technology requires thickened areas on each metallized layer, requiring staggered edges during component rolling, which increases component length by 1-1.3mm. This makes it suitable for films with smaller widths but less suitable for films with widths of 150μm.
[0008] Document CN 103366958A discloses a high-voltage metallized film capacitor, primarily designed for 10kV high-voltage electrical energy metering devices. This AC capacitor features a multi-segment internal series structure, offering high output voltage, small size, and compact structure. However, this technology has several drawbacks: The multi-segment internal series structure results in an effective electrode width of 2-4mm. The offset between the two metallized films during winding affects the capacitance deviation and voltage divider ratio; the electrode square resistance is 7-10Ω / □, and the operating field strength is also relatively low.
[0009] Although the metallized film with the multi-string structure has advantages such as high current density, small size, and reduced processing steps, its main sheet resistance is low and the working field strength is low, so it is not suitable for high-voltage DC support capacitors with high working field strength.
[0010] In summary, the key considerations for metallized films used in high-voltage DC support capacitors include: internal series structure; square resistance structure; film thickness; and operating field strength. Addressing these key technologies is crucial for the development of this type of metallized film. Summary of the Invention
[0011] In order to overcome the technical shortcomings of the existing metallized film of DC support capacitors, the present invention provides a metallized film for high-voltage dry-type DC support capacitors.
[0012] The technical solutions adopted by the present invention are as follows.
[0013] The present invention provides a metallized film for a high-voltage dry-type DC support capacitor. The metallized film mainly comprises a first metallized film layer and a second metallized film layer. The first metallized film layer comprises a first base film and a first vapor-deposited layer. The second metallized film layer comprises a second base film and a second vapor-deposited layer.
[0014] The first evaporated layer consists of a first edge thickening area, a first active area, a second active area, a first intermediate screen strip, a third active area, a fourth active area, and a second edge thickening area. The first edge thickening area is horizontally connected to the first active area, the first active area is horizontally connected to the second active area, the first intermediate screen strip is horizontally connected between the second and third active areas, the third active area is horizontally connected to the fourth active area, and the fourth active area is horizontally connected to the second edge thickening area.
[0015] The second evaporated layer consists of a first edge screen band, the fifth active area, the sixth active area, the seventh active area, a second intermediate screen band, the eighth active area, and a second edge screen band. The first edge screen band is horizontally connected to the fifth active area, the sixth active area is horizontally connected between the fifth and seventh active areas, the second intermediate screen band is horizontally connected between the seventh and eighth active areas, and the eighth active area is horizontally connected to the second edge screen band.
[0016] When the first metallized film layer and the second metallized film layer are superimposed, the first intermediate screen belt and the second intermediate screen belt separate the first vapor-deposited layer and the second vapor-deposited layer for a second time, and are equivalent to a three-string structure with equal capacitance value.
[0017] The first base film is a high-temperature resistant electrical polypropylene film with a width of 100~150mm and a maximum working temperature of 110℃.
[0018] The second base film is a high-temperature resistant electrical polypropylene film with a width of 98~148mm and a maximum operating temperature of 110℃.
[0019] The width of the first edge thickened area is 5 mm, the sheet resistance of the evaporated metal layer is 2 (1-3) Ω / □, and the material thereof is zinc-aluminum alloy.
[0020] The sheet resistance of the metal layer evaporated in the first active area is 7 (5-9) Ω / □, and the material thereof is zinc-aluminum alloy.
[0021] The sheet resistance of the metal layer evaporated in the second active area is 50 (40-60) Ω / □, and the material thereof is zinc-aluminum alloy.
[0022] The width of the first intermediate screen strip is 5 mm.
[0023] The sheet resistance of the metal layer evaporated in the third active area is 50 (40-60) Ω / □, and the material thereof is zinc-aluminum alloy.
[0024] The sheet resistance of the metal layer deposited in the fourth active area is 7 (5-9) Ω / □, and the material thereof is zinc-aluminum alloy.
[0025] The width of the second edge thickened area is 5 mm, the sheet resistance of the evaporated metal layer is 2 (1-3) Ω / □, and the material thereof is zinc-aluminum alloy.
[0026] The width of the first edge screen band is 2.5~3mm.
[0027] The sheet resistance of the metal layer deposited on the fifth active area is 50 (40-60) Ω / □, and the material thereof is zinc-aluminum alloy.
[0028] The sheet resistance of the metal layer deposited on the sixth active area is 7 (5-9) Ω / □, and the material thereof is zinc-aluminum alloy.
[0029] The metal layer evaporated in the seventh active area has a square resistance of 50 (40-60) Ω / □ and is made of zinc-aluminum alloy.
[0030] The width of the second intermediate screen strip is 5 mm.
[0031] The sheet resistance of the metal layer deposited in the eighth active area is 40 (30-50) Ω / □, and the material thereof is zinc-aluminum alloy.
[0032] Furthermore, the first base film is 2 mm wider than the second base film, and the thickness and material of the two are the same. Under special operating conditions, the two can also have different thicknesses.
[0033] Furthermore, the width of the first active area accounts for about 10% of the width of the first base film, the width of the second active area accounts for about 28% of the width of the first base film, the width of the third active area accounts for about 51% of the width of the first base film, and the width of the fourth active area accounts for about 10% of the width of the first base film.
[0034] Furthermore, the width of the fifth active area accounts for about 25% of the width of the first base film, the width of the sixth active area accounts for about 19% of the width of the first base film, the width of the seventh active area accounts for about 25% of the width of the first base film, and the width of the eighth active area accounts for about 30% of the width of the first base film.
[0035] The beneficial effects of the present invention are: in addition to the advantages of the inner-series structure metallized film having a high current density, a small volume, and reduced processing steps, the use of a thin metallized film with three inner-series structures can achieve a capacitor operating field strength of 240V / µm, reduce the size of the capacitor, and improve its self-healing properties.
[0036] The present invention has a simple structure and is easy to manufacture, and can meet the high-voltage DC support capacitor's high long-term safe and reliable operation requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a schematic diagram of the present invention; Figure 2 is a side view of the first layer of metallized film; Figure 3 is a side view of the second metallized film; Figure 4 Equivalent circuit diagram for the application of the present invention; 11-first base film; 12-first vapor-deposited layer; 21-second base film; 22-second vapor-deposited layer; 121 - first edge thickening area; 122 - first active area; 123 - second active area; 124 - first intermediate screen band; 125 - third active area; 126 - fourth active area; 127 - second edge thickening area; 221 - first edge screen band; 222 - fifth active area; 223 - sixth active area; 224 - seventh active area; 225 - second middle screen band; 226 - eighth active area; 227 - second edge screen band. DETAILED DESCRIPTION
[0038] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0039] exist Figure 1It can be seen that the metallized film for high-voltage dry-type DC support capacitors is mainly composed of a first metallized film (1) and a second metallized film (2); the first metallized film (1) is composed of a first base film (11) and a first vapor-deposited layer (12); the second metallized film (2) is composed of a second base film (21) and a second vapor-deposited layer (22).
[0040] exist Figure 2 It can be seen that the first vapor-deposited layer (12) is composed of a first edge thickening area (121), a first active area (122), a second active area (123), a first intermediate screen band (124), a third active area (125), a fourth active area (126), and a second edge thickening area (127); the first edge thickening area (121) is horizontally connected to the first active area (122), the first active area (122) is horizontally connected to the second active area (123), the first intermediate screen band (124) is horizontally connected between the second active area (123) and the third active area (125), the third active area (125) is horizontally connected to the fourth active area (126), and the fourth active area (126) is horizontally connected to the second edge thickening area (127).
[0041] exist Figure 3 It can be seen that the second vapor-deposited layer (22) is composed of a first edge screen band (221), a fifth active area (222), a sixth active area (223), a seventh active area (224), a second intermediate screen band (225), an eighth active area (226), and a second edge screen band (227); the first edge screen band (221) is horizontally connected to the fifth active area (222), the sixth active area (223) is horizontally connected between the fifth active area (222) and the seventh active area (224), the second intermediate screen band (225) is horizontally connected between the seventh active area (224) and the eighth active area (226), and the eighth active area (226) is horizontally connected to the second edge screen band (227).
[0042] exist Figure 4 It can be seen that after the first metallized film (1) and the second metallized film (2) are superimposed, the first intermediate screen strip (124) and the second intermediate screen strip (225) separate the first vapor-deposited layer (1) and the second vapor-deposited layer (2) for a second time, and are equivalent to a three-string structure with equal capacitance value.
[0043] The first base film (11) is a high-temperature resistant electrical polypropylene film with a width of 100-150 mm and a maximum operating temperature of 110°C.
[0044] The second base film (21) is a high-temperature resistant electrical polypropylene film with a width of 98-148 mm and a maximum operating temperature of 110°C.
[0045] The first edge thickening area (121) has a width of 5 mm, and the sheet resistance of the evaporated metal layer is 2 (1-3) Ω / □, and the material thereof is a zinc-aluminum alloy.
[0046] The sheet resistance of the metal layer deposited in the first active area (122) is 7 (5-9) Ω / □, and the material thereof is a zinc-aluminum alloy.
[0047] The metal layer evaporated in the second active area (123) has a square resistance of 50 (40-60) Ω / □ and is made of zinc-aluminum alloy.
[0048] The first intermediate screen strip (124) has a width of 5 mm.
[0049] The metal layer evaporated in the third active area (125) has a square resistance of 50 (40-60) Ω / □ and is made of zinc-aluminum alloy.
[0050] The metal layer evaporated in the fourth active area (126) has a square resistance of 7 (5-9) Ω / □ and is made of zinc-aluminum alloy.
[0051] The width of the second edge thickened area (127) is 5 mm, the square resistance of the evaporated metal layer is 2 (1-3) Ω / □, and the material thereof is zinc-aluminum alloy.
[0052] The first edge screen strip (221) has a width of 2.5-3 mm.
[0053] The metal layer evaporated in the fifth active area (222) has a square resistance of 50 (40-60) Ω / □ and is made of zinc-aluminum alloy.
[0054] The metal layer evaporated in the sixth active area (223) has a square resistance of 7 (5-9) Ω / □ and is made of zinc-aluminum alloy.
[0055] The metal layer evaporated in the seventh active area (224) has a square resistance of 50 (40-60) Ω / □ and is made of zinc-aluminum alloy.
[0056] The width of the second intermediate screen strip (225) is 5 mm.
[0057] The metal layer evaporated in the eighth active area (226) has a square resistance of 40 (30-50) Ω / □ and is made of zinc-aluminum alloy.
[0058] The first edge screen strip (227) has a width of 2.5-3 mm.
[0059] Furthermore, the first base film (11) is 2 mm wider than the second base film (21), and the thickness and material of the two are the same. Under special operating conditions, the two can also have different thicknesses.
[0060] Furthermore, the width of the first active area (122) accounts for approximately 10% of the width of the first base film (11), the width of the second active area accounts for approximately 28% of the width of the first base film (11), the width of the third active area accounts for approximately 51% of the width of the first base film (11), and the width of the fourth active area (11) accounts for approximately 10% of the width of the first base film.
[0061] Furthermore, the width of the fifth active area (222) accounts for approximately 25% of the width of the second base film (21), the width of the sixth active area (223) accounts for approximately 19% of the width of the second base film (21), the width of the seventh active area (224) accounts for approximately 25% of the width of the second base film (21), and the width of the eighth active area (226) accounts for approximately 30% of the width of the second base film (21).
[0062] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included in the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.
Claims
1. A metallized film for a high-voltage dry-type DC support capacitor, characterized by: The metallized film mainly consists of a first metallized film layer and a second metallized film layer, wherein the first metallized film layer consists of a first base film and a first vapor-deposited layer, and the second metallized film layer consists of a second base film and a second vapor-deposited layer; The first evaporated layer is composed of a first edge thickening area, a first active area, a second active area, a first intermediate screen band, a third active area, a fourth active area, and a second edge thickening area. The first edge thickening area is horizontally connected to the first active area, the first active area is horizontally connected to the second active area, the first intermediate screen band is horizontally connected between the second active area and the third active area, the third active area is horizontally connected to the fourth active area, and the fourth active area is horizontally connected to the second edge thickening area. The second evaporated layer is composed of a first edge screen band, a fifth active area, a sixth active area, a seventh active area, a second intermediate screen band, an eighth active area, and a second edge screen band, wherein the first edge screen band is horizontally connected to the fifth active area, the sixth active area is horizontally connected between the fifth active area and the seventh active area, the second intermediate screen band is horizontally connected between the seventh active area and the eighth active area, and the eighth active area is horizontally connected to the second edge screen band; After the first metallized film layer and the second metallized film layer are stacked, the first intermediate screen belt and the second intermediate screen belt separate the first vapor-deposited layer and the second vapor-deposited layer for a second time and form an equivalent three-string structure.
2. The metallized film according to claim 1, wherein: The width of the first edge thickened area is 5 mm, the sheet resistance of the evaporated metal layer is 2 (1-3) Ω / □, and the material thereof is zinc-aluminum alloy.
3. The metallized film according to claim 1, wherein: The metal layer evaporated in the first active area has a square resistance of 7 (5-9) Ω / □ and is made of zinc-aluminum alloy.
4. The metallized film according to claim 1, wherein: The sheet resistance of the metal layer evaporated in the second active area is 50 (40-60) Ω / □, and the material thereof is zinc-aluminum alloy.
5. The metallized film according to claim 1, wherein: The sheet resistance of the metal layer evaporated in the third active area is 50 (40-60) Ω / □, and the material thereof is zinc-aluminum alloy.
6. The metallized film according to claim 1, wherein: The sheet resistance of the metal layer evaporated in the fourth active area is 7 (5-9) Ω / □, and the material thereof is zinc-aluminum alloy.
7. The metallized film according to claim 1, wherein: The sheet resistance of the metal layer evaporated in the fifth active area is 50 (40-60) Ω / □, and the material thereof is zinc-aluminum alloy.
8. The metallized film according to claim 1, wherein: The sheet resistance of the metal layer evaporated in the sixth active area is 7 (5-9) Ω / □, and the material thereof is zinc-aluminum alloy.
9. The metallized film according to claim 1, wherein: The metal layer evaporated in the seventh active area has a square resistance of 50 (40-60) Ω / □, and its material is zinc-aluminum alloy.
10. The metallized film according to claim 1, wherein: The sheet resistance of the metal layer evaporated in the eighth active area is 40 (30-50) Ω / □, and the material thereof is zinc-aluminum alloy.
Citation Information
Patent Citations
High-voltage metallized film capacitor
CN103366958A
Metalized thin film with multiple inner string structures
CN108597866A