Surface treatment method of TCO (Transparent Conductive Oxide) film layer
By hydroxylating the TCO film layer and depositing a silane coupling agent layer, the problem of poor wettability between the TCO film layer and the low-temperature solder tape was solved, low contact resistance and high mechanical bonding strength were achieved, and battery performance was improved.
Patent Information
- Application Number
- CN202510822535.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-18
- Publication Date
- 2025-09-09
AI Technical Summary
The TCO film layer has low surface energy and poor wettability with low-temperature solder strips, resulting in high interface contact resistance and weak mechanical bonding, affecting battery efficiency and component reliability.
The TCO film layer is subjected to surface hydroxylation treatment, and a silane coupling agent (SAM) layer is deposited. The surface of the film layer is covered with hydroxyl groups through a chemical vapor or UV ozone process, and silane coupling agent molecules are deposited in a vacuum chamber to form a dense monolayer.
The contact angle between the TCO film layer and the low-temperature solder tape is significantly reduced, the wettability and spreadability are improved, the mechanical bonding force is enhanced, the interface contact resistance is reduced, and the battery efficiency and component stability are improved.
Smart Images

Figure CN120614894A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a surface treatment method for a TCO film layer. Background Art
[0002] In the solar cell field, busbar-less (OBB) technology has emerged to reduce silver paste raw material costs and minimize shading losses. Currently, mainstream OBB technologies include SmartWire, UV dispensing, and solder dispensing. However, these technologies only achieve effective connections between the low-temperature solder ribbon and the metal sub-grid, but fail to achieve a good alloying between the low-temperature solder ribbon and the transparent conductive oxide (TCO) film. This makes it difficult to further reduce contact resistance, thus affecting cell efficiency.
[0003] To further optimize cell structure, reduce costs, and minimize shading losses, sidebar-free OBB technology has become a new research hotspot. This technology abandons traditional sidebar designs and relies solely on direct contact between a low-temperature solder ribbon and the TCO film to achieve current collection and conduction. However, the low surface energy of the TCO film leads to poor wettability with the low-temperature solder ribbon (low-temperature solder or conductive adhesive), which can easily lead to high interfacial contact resistance and weak mechanical bonding, resulting in reduced cell efficiency and module reliability issues such as debonding and hidden cracks. Therefore, how to treat the TCO film surface to improve its wettability and bonding with the low-temperature solder ribbon has become a pressing technical challenge. Summary of the Invention
[0004] Based on this, the present application provides a surface treatment method for a TCO film layer to solve the above technical problems.
[0005] A surface treatment method for a TCO film layer comprises the following steps:
[0006] Performing surface hydroxylation treatment on the TCO film layer to obtain a hydroxylated TCO film layer;
[0007] A silane coupling agent (SAM) layer is deposited on the hydroxylated TCO film layer.
[0008] In some embodiments, the TCO film layer is subjected to surface hydroxylation treatment using a chemical vapor treatment process or an ultraviolet ozonation process; wherein,
[0009] The chemical vapor treatment process includes the following steps: placing the TCO film layer in a process chamber, continuously introducing ozone and water vapor into the process chamber for a reaction time of 5 to 30 minutes at a substrate temperature of 60°C to 120°C, so that the surface of the TCO film layer is covered with hydroxyl groups;
[0010] The UV ozone oxidation process includes the following steps: placing the TCO film layer in a UV ozone machine with a UV lamp power density of 20mW / cm 2 The reaction time is 15 min to 30 min, so that the surface of the TCO film is covered with hydroxyl groups.
[0011] In some embodiments, the silane coupling agent (SAM) layer is deposited by chemical vapor deposition or solution deposition.
[0012] In some embodiments, the chemical vapor deposition method includes the following steps:
[0013] The hydroxylated TCO film layer is placed in a vacuum chamber, into which silane coupling agent molecules and water molecules are introduced simultaneously, with a molar ratio of the silane coupling agent molecules to the water molecules being 1:(2~10), a deposition time being 2min~30min, and a substrate temperature being 50°C~120°C.
[0014] In some embodiments, silane coupling agent molecules and water molecules are introduced simultaneously within a first preset time; nitrogen is introduced to purge the vacuum chamber within a second preset time; and the above steps are alternately performed N times.
[0015] In some embodiments, before introducing nitrogen, the method further comprises the following steps: evacuating the vacuum chamber to below 1 Pa.
[0016] In some embodiments, the solution deposition method includes at least one of dip coating, slot coating, drop coating, spin coating, doctor blade coating, roller coating, spray coating, and inkjet printing.
[0017] In some embodiments, the surface treatment method of the TCO film layer further includes a curing step, curing the TCO film layer deposited with the silane coupling agent (SAM) layer at 80° C. to 120° C. for 2 min to 30 min.
[0018] In some embodiments, the silane coupling agent (SAM) layer is a monolayer.
[0019] In some embodiments, the silane coupling agent (SAM) layer includes a silane coupling agent material having the chemical formula RSiX3, wherein:
[0020] R includes at least one of vinyl, amino, epoxy, methacryloxy, mercapto, and urea groups;
[0021] X includes at least one of a chloro group, a methoxy group, an ethoxy group, a methoxyethoxy group, and an acetoxy group.
[0022] In some embodiments, R is at least one of an amino group, a thiol group, and a urea group.
[0023] The present application deposits a self-assembled layer of silane coupling agent on the TCO film layer to regulate the chemical properties of the TCO film surface, thereby significantly reducing the contact angle between the TCO film layer and the low-temperature solder strip, improving the wettability between the TCO film layer and the solder on the surface of the low-temperature solder strip, improving the spreading of the solder on the surface of the low-temperature solder strip on the TCO film layer, reducing the void rate, improving the mechanical bonding force between the two, reducing the interface contact resistance, and improving the battery efficiency and component stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application or related technologies, the following briefly introduces the drawings required for use in the embodiments or related technical descriptions. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0025] Figure 1 This is an SEM image of the TCO film layer and the low-temperature solder tape after lamination in Example 1.
[0026] Figure 2 This is an SEM image of the TCO film layer and the low-temperature solder tape after lamination in Comparative Example 1. DETAILED DESCRIPTION
[0027] Reference will now be made to embodiments of the present application in detail, one or more examples of which are described below. Each example is provided to illustrate, but not to limit, the present application. Indeed, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, features illustrated or described as part of one embodiment may be used in another embodiment to produce further embodiments.
[0028] Therefore, it is intended that this application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features, and aspects of the present application are disclosed in or are apparent from the following detailed description. Those skilled in the art will appreciate that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.
[0029] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0030] In this application, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.
[0031] In this document, when referring to a range, if the unit is followed only by the right endpoint, it means that the units of the left and right endpoints are the same. For example, 100~150nm means that the units of the left endpoint "100" and the right endpoint "150" are both nm (nanometers).
[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0034] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a statement that a method includes steps (a) and (b) indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a statement that a method may also include step (c) indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.
[0035] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.
[0036] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0037] Transparent conductive oxide (TCO) layers (such as ITO and IWO) have low surface energy and poor wettability with non-high-temperature solder strips (low-temperature solder or conductive adhesive). This results in high interfacial contact resistance and weak mechanical bonding, which can easily lead to battery efficiency loss and component reliability issues (such as grid delamination and hidden cracks). Based on this, this application provides a surface treatment method for TCO film layers to address the above-mentioned technical problems.
[0038] A surface treatment method for a TCO film layer comprises the following steps:
[0039] Performing surface hydroxylation treatment on the TCO film layer to obtain a hydroxylated TCO film layer;
[0040] A silane coupling agent (SAM) layer is deposited on the hydroxylated TCO film layer.
[0041] The present application deposits a self-assembled layer of silane coupling agent on the TCO film layer to regulate the chemical properties of the TCO film surface, thereby significantly reducing the contact angle between the TCO film layer and the low-temperature solder strip, improving the wettability between the TCO film layer and the solder on the surface of the low-temperature solder strip, improving the spreading of the solder on the surface of the low-temperature solder strip on the TCO film layer, reducing the void rate, improving the mechanical bonding force between the two, reducing the interface contact resistance, and improving the battery efficiency and component stability.
[0042] In some embodiments, the surface of the TCO film layer is hydroxylated by using a chemical vapor treatment process or an ultraviolet ozonation process.
[0043] The chemical vapor treatment process includes the following steps: placing the TCO film layer in a process chamber, continuously introducing ozone and water vapor into the process chamber, with a molar ratio of ozone to water vapor of (1:2) to (2:1), a reaction time of 5 minutes to 30 minutes, and a substrate temperature of 60°C to 120°C, so that the surface of the TCO film layer is covered with hydroxyl groups.
[0044] In some embodiments, the process chamber is a vacuum chamber (pressure ≤ 1 Pa). In this application, the chemical vapor treatment process performed in a vacuum chamber is referred to as a "vacuum process."
[0045] The UV ozone oxidation process includes the following steps: placing the TCO film layer in a UV ozone machine with a UV lamp power density of 20mW / cm 2 The reaction time is 15 min to 30 min, so that the surface of the TCO film is covered with hydroxyl groups.
[0046] Before the silane coupling agent (SAM) layer deposition step is performed in the present application, the surface of the TCO film layer is first subjected to a hydroxylation treatment, so that a sufficient number of hydroxyl groups are distributed on the surface of the TCO film layer. Through the chemical bonding between the hydroxyl groups and the silanol groups generated by the hydrolysis of the silane coupling agent molecules, the silane coupling agent is firmly attached to the surface of the TCO film layer, thereby avoiding the shedding of the silane coupling agent during use and improving the interface stability.
[0047] In some embodiments, the silane coupling agent (SAM) layer is deposited by chemical vapor deposition or solution deposition.
[0048] In some embodiments, the chemical vapor deposition method includes the following steps:
[0049] The hydroxylated TCO film layer is placed in a vacuum chamber (pressure ≤ 1 Pa). In the vacuum chamber, silane coupling agent molecules and water molecules are introduced simultaneously. The molar ratio of the silane coupling agent molecules to the water molecules is 1: (2~10). The deposition time is 2min~30min and the substrate temperature is 50℃~120℃.
[0050] In some embodiments, silane coupling agent molecules and water molecules are introduced simultaneously within a first preset time; nitrogen is introduced to purge the vacuum chamber within a second preset time; and the above steps are alternately performed N times.
[0051] In some embodiments, the first preset time is 0.01s~10s, including but not limited to 0.01s, 1s, 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, and 10s.
[0052] In some embodiments, the second preset time is 3s~120s, including but not limited to 3s, 10s, 20s, 25s, 30s, 35s, 40s, 50s, 70s, 90s, 100s, and 120s.
[0053] It is understandable that the first preset time and the second preset time in this application may be the same or different.
[0054] Exemplarily, the chemical vapor deposition method includes the following steps:
[0055] Silane coupling agent molecules and water molecules were introduced simultaneously into the vacuum chamber for 1 second, followed by nitrogen gas for 10 seconds to purge the chamber. These steps were repeated 20 times. The molar ratio of silane coupling agent molecules to water molecules was 1:2, and the substrate temperature was 80°C.
[0056] Since there are unbonded silane coupling agent molecules on the surface of the chamber and the substrate, the unbonded silane coupling agent molecules will occupy steric hindrance and affect the growth of the area not covered by the silane coupling agent. Therefore, the present application intermittently introduces nitrogen to purge and remove the silane coupling agent molecules that have not grown on the surface of the chamber and the substrate, thereby reducing the subsequent growth steric hindrance and completing the growth of a dense monolayer on the surface of the TCO film layer.
[0057] In some embodiments, before introducing nitrogen, the method further comprises the following steps: evacuating the vacuum chamber to below 1 Pa.
[0058] By adding a vacuum step before the nitrogen injection step to remove residual gas from the chamber, the removal of unbonded silane coupling agent molecules in the chamber is enhanced, further reducing the subsequent growth hindrance and ensuring the growth of a dense monolayer on the surface of the TCO film. This application uses chemical vapor deposition to deposit the silane coupling agent (SAM) layer, which has good uniformity and is suitable for mass production.
[0059] In some embodiments, the solution deposition method includes at least one of dip coating, slot coating, drop coating, spin coating, doctor blade coating, roller coating, spray coating, and inkjet printing.
[0060] Exemplarily, the dip coating method includes the following steps:
[0061] The TCO film layer is immersed in a solution containing a silane coupling agent, wherein the solvent of the solution is an ethanol / water mixed system (the volume ratio of ethanol to water is 9:1).
[0062] The concentration of the silane coupling agent solution is 0.0001wt%~5wt%, including but not limited to 0.0001wt%, 0.1wt%, 1wt%, 2wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, and 5wt%.
[0063] The processing time is 5min~60min, including but not limited to 5min, 10min, 20min, 30min, 40min, 50min, and 60min.
[0064] The processing temperature is 20°C~60°C, including but not limited to 20°C, 30°C, 40°C, 50°C, and 60°C.
[0065] In some embodiments, while immersing the TCO film layer in a solution containing a silane coupling agent, ultrasonic treatment is simultaneously performed to disperse the silane coupling agent in the solution, prevent molecular clustering, and remove unreacted silane coupling agent molecules on the substrate surface.
[0066] Exemplarily, slot coating comprises the following steps:
[0067] A silane coupling agent solution is slit-coated on the surface of the TCO film. The solvent of the solution is an ethanol / water mixture (the volume ratio of ethanol to water is 9:1). The concentration of the silane coupling agent solution is 0.0001wt% to 5wt%, including but not limited to 0.0001wt%, 0.01wt%, 0.1wt%, 1wt%, 2wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, and 5wt%.
[0068] The present application adopts a solution deposition method to deposit the silane coupling agent (SAM) layer, which is low-cost and suitable for mass production.
[0069] In some embodiments, the surface of the TCO film layer is hydroxylated using a vacuum process, and the silane coupling agent layer is deposited using a chemical vapor deposition method.
[0070] During the hydroxylation process, when a vacuum process is used, the vacuum heating environment will cause the hydroxyl groups to desorb after growing on the surface of the TCO film layer. Therefore, the present application uses a vacuum process combined with a chemical vapor deposition method to complete the surface treatment of the TCO film layer. After the hydroxylation treatment in the vacuum process is completed, the deposition of the silane coupling agent in the next step is quickly completed in the same vacuum chamber, thereby avoiding the desorption of hydroxyl groups on the surface of the TCO film layer during the vacuum process.
[0071] In some embodiments, the surface of the TCO film layer is hydroxylated by using an ultraviolet ozonation process, and the silane coupling agent layer is deposited by using a solution deposition method.
[0072] In some embodiments, the surface treatment method of the TCO film layer further includes a curing step, removing the surface solution by blowing dry, and curing the TCO film layer deposited with the silane coupling agent (SAM) layer at 80° C. to 120° C. for 2 min to 30 min.
[0073] It is understandable that when the silane coupling agent (SAM) layer is deposited by chemical vapor deposition, the above-mentioned curing step is not required. When the silane coupling agent (SAM) layer is deposited only by solution deposition, the above-mentioned curing step is required.
[0074] In some embodiments, before the TCO film layer is subjected to the hydroxylation treatment, a cleaning step is further included: the TCO film layer is cleaned to remove contaminants on the surface of the TCO film layer.
[0075] For example, the TCO film layer is cleaned by ultrasonic cleaning with deionized water.
[0076] It is understood that if the TCO film is newly prepared, no cleaning step is required. In some embodiments, the silane coupling agent (SAM) layer is a monolayer.
[0077] It can be understood that the silane coupling agent (SAM) layer being a monomolecular layer means that the thickness of the silicon-based coupling agent layer is equal to the size of the silicon-based coupling agent molecules used.
[0078] In some embodiments, the silane coupling agent (SAM) layer includes a silane coupling agent material having a chemical formula of RSiX3, wherein:
[0079] R represents an organic functional group, including but not limited to at least one of vinyl, amino, epoxy, methacryloxy, mercapto, and urea;
[0080] X represents a hydrolyzable functional group, including but not limited to at least one of chloro, methoxy, ethoxy, methoxyethoxy, and acetoxy.
[0081] In a preferred embodiment, R is at least one of an amino group, a thiol group, and a urea group.
[0082] The surface treatment method provided in this application significantly reduces the contact angle between the TCO film layer and the low-temperature solder tape, improves the spreadability of the low-temperature solder tape, reduces the void rate, and greatly reduces the interface resistance. The low interface contact resistance can still be maintained after high and low temperature cycle aging.
[0083] The surface treatment method provided in this application adopts low-temperature treatment (≤120°C) to avoid damaging the passivation layer of the HJT battery and the perovskite layer of the stacked battery.
[0084] The silane coupling agent (SAM) layer deposited on the surface of the TCO film layer in this application has high chemical stability and excellent resistance to moisture and heat aging.
[0085] The present application will be further described below with reference to specific embodiments.
[0086] Example 1
[0087] Cleaning step: The TCO film layer of the crystalline silicon cell or stacked cell is subjected to ultrasonic cleaning treatment with deionized water to remove pollutants on the surface of the TCO film layer.
[0088] Hydroxylation treatment: The TCO film layer is placed in a vacuum chamber (pressure ≤ 1Pa), and ozone and water vapor (the molar ratio of ozone to water vapor is 1:1) are continuously introduced for 5 minutes at a substrate temperature of 100°C to make the surface of the TCO film layer covered with hydroxyl groups.
[0089] Silane coupling agent (SAM) layer deposition: The hydroxylated TCO film is placed in a vacuum chamber (pressure ≤ 1 Pa). Silane coupling agent molecules and water molecules are introduced simultaneously into the chamber. The molar ratio of silane coupling agent to water molecules is 1:2. The deposition time is 8 minutes, and the substrate temperature is 100°C. At this point, the silanol groups generated by the hydrolysis of the silane coupling agent react with the hydroxyl groups distributed on the surface of the TCO film to form siloxane, forming a uniform silane coupling agent layer on the surface of the TCO film.
[0090] Post-processing steps: vacuum remove residual gas, remove unbonded molecules in the vacuum chamber, and introduce nitrogen to break the air.
[0091] Example 2
[0092] The difference between this embodiment and embodiment 1 is that the silane coupling agent (SAM) layer deposition step is different.
[0093] Silane coupling agent (SAM) layer deposition: The TCO film is placed in a vacuum chamber (pressure ≤ 1 Pa), and silane coupling agent molecules and water molecules are introduced simultaneously for 1 second. Nitrogen gas is then introduced for 10 seconds, and the vacuum chamber is purged. This process is repeated 20 times. The molar ratio of silane coupling agent molecules to water molecules is 1:10, and the substrate temperature is 120°C. During this process, the silanol groups generated by the hydrolysis of the silane coupling agent react with the hydroxyl groups distributed on the surface of the TCO film to form siloxane, forming a uniform silane coupling agent layer on the surface of the TCO film.
[0094] Example 3
[0095] Cleaning step: The TCO film layer of the HJT battery is ultrasonically cleaned with deionized water to remove contaminants on the surface of the TCO film layer.
[0096] Hydroxylation treatment: Place the TCO film layer in a UV ozone machine to make the surface of the TCO film layer covered with hydroxyl groups. The power density of the UV lamp in the UV ozone machine is 30mW / cm 2 , the reaction time is 30min.
[0097] Silane coupling agent (SAM) layer deposition: The hydroxylated TCO film was immersed in a 0.0001 wt% silane coupling agent solution in an ethanol / water mixture (9:1 volume ratio) for 5 minutes at 60°C.
[0098] Curing step: remove the surface solution by blowing dry, and cure at 120℃ for 5 minutes.
[0099] Example 4
[0100] Cleaning step: The TCO film layer of the HJT battery is ultrasonically cleaned with deionized water to remove contaminants on the surface of the TCO film layer.
[0101] Hydroxylation treatment: Place the TCO film layer in a UV ozone machine to make the surface of the TCO film layer covered with hydroxyl groups. The power density of the UV lamp of the UV ozone machine is 25mW / cm 2 , the reaction time is 20min.
[0102] Silane coupling agent (SAM) layer deposition: A silane coupling agent solution (0.001 wt%) was slit-coated on the surface of the hydroxylated TCO film. The solvent of the solution was an ethanol / water mixture (9:1 by volume).
[0103] Curing step: Curing at 120°C for 20 minutes.
[0104] Comparative Example 1
[0105] A TCO film layer that has only been cleaned was selected as a comparative example.
[0106] Test Case
[0107] The following performance tests were performed on the surface-treated TCO film layers in the examples and comparative examples.
[0108] (1) Interface contact resistance test
[0109] Low-temperature solder ribbon was laminated onto a crystalline silicon surface with a TCO / SiO2 film using a laminator, glass, and adhesive film. The SiO2 layer served as an insulating layer to ensure the silicon's conductivity did not interfere with the test. The solder ribbons were arranged parallel to each other with spacings of 1, 2, 3, 4, 5, 6, 7, and 8 mm. A precision source meter was used to measure the resistance of each pair of adjacent ribbons, and the interfacial contact resistance between the low-temperature solder ribbon and the TCO film was calculated using the TLM method.
[0110] (2) Hygrothermal aging performance test
[0111] The interface contact resistance test samples were placed in a test chamber (environmental conditions: -30°C to 85°C high and low temperature cycling). The chamber was operated continuously for the specified time (50 cycles). The appearance of the samples was regularly observed for changes. After the aging period, the interface contact resistance was tested again. The results are shown in Table 1 below.
[0112] Table 1
[0113]
[0114] Compared with Comparative Example 1, the interface contact resistance of the TCO film layer treated by the surface treatment method provided in the present application is greatly reduced, and the interface contact resistance can still be maintained at a low level after high and low temperature cycle aging.
[0115] (3) SEM test
[0116] The treated TCO films in Example 1 and Comparative Example 1 were selected as test objects, and were laminated with low-temperature solder tapes, and then scanned by electron microscope. Figure 1 As stated, Figure 1 This is an SEM image of the TCO film layer and the low-temperature solder tape after lamination in Example 1. Figure 2 This is an SEM image of the TCO film layer and the low-temperature solder tape after lamination in Comparative Example 1.
[0117] according to Figure 1 It can be seen that after the TCO film layer is deposited with silane coupling agent, the low-temperature alloy on the surface of the low-temperature solder strip after lamination can fully infiltrate the pyramid valley bottom on the surface of the silicon wafer. Figure 2 It can be seen that when the TCO film layer is not treated with silane coupling agent deposition, a large number of voids are present in the low-temperature alloy on the surface of the low-temperature solder tape and the pyramid valleys on the surface of the silicon wafer after lamination. This shows that the surface treatment method of the present application significantly reduces the void rate.
[0118] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0119] The above embodiments merely illustrate several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A surface treatment method for a TCO film layer, characterized in that: The following steps are involved: Performing surface hydroxylation treatment on the TCO film layer to obtain a hydroxylated TCO film layer; A silane coupling agent layer is deposited on the hydroxylated TCO film layer.
2. The surface treatment method of the TCO film layer according to claim 1, characterized in that: The TCO film layer is subjected to surface hydroxylation treatment by using a chemical vapor treatment process or an ultraviolet ozonation process; wherein, The chemical vapor treatment process comprises the following steps: placing the TCO film layer in a process chamber, continuously introducing ozone and water vapor into the process chamber for a reaction time of 5 minutes to 30 minutes and a substrate temperature of 60° C. to make the surface of the TCO film layer covered with hydroxyl groups; The UV ozonation process includes the following steps: placing the TCO film layer in a UV ozone machine with a UV lamp power density of 20 mW / cm 2 The reaction time is 15 min to 30 min, so that the surface of the TCO film is covered with hydroxyl groups.
3. The surface treatment method of the TCO film layer according to claim 1, characterized in that: The silane coupling agent layer is deposited by chemical vapor deposition or solution deposition.
4. The surface treatment method of the TCO film layer according to claim 3, characterized in that: The chemical vapor deposition method comprises the following steps: The hydroxylated TCO film layer is placed in a vacuum chamber, and silane coupling agent molecules and water molecules are introduced into the vacuum chamber at the same time, wherein the molar ratio of the silane coupling agent molecules to the water molecules is 1:(2-10), the deposition time is 2 min-30 min, and the substrate temperature is 50° C.-120° C.
5. The surface treatment method of the TCO film layer according to claim 4, characterized in that: During a first preset time, silane coupling agent molecules and water molecules are introduced simultaneously; during a second preset time, nitrogen is introduced to purge the vacuum chamber, and the above steps are alternately performed N times.
6. The surface treatment method of the TCO film layer according to claim 5, characterized in that: Before introducing nitrogen, the method further comprises the following steps: evacuating the vacuum chamber to below 1 Pa.
7. The surface treatment method of the TCO film layer according to claim 3, characterized in that: The solution deposition method includes at least one of dip coating, slot coating, drop coating, spin coating, doctor blade coating, roller coating, spray coating, and inkjet printing.
8. The surface treatment method of the TCO film layer according to claim 7, characterized in that: The surface treatment method of the TCO film layer also includes a curing step, wherein the TCO film layer deposited with the silane coupling agent layer is cured at 80° C. to 120° C. for 2 min to 30 min.
9. The surface treatment method of the TCO film according to any one of claims 1 to 8, characterized in that: The silane coupling agent layer is a monomolecular layer.
10. The surface treatment method of the TCO film according to any one of claims 1 to 8, characterized in that: The silane coupling agent layer includes a silane coupling agent material having a chemical formula of RSiX3, wherein: R includes at least one of vinyl, amino, epoxy, methacryloxy, mercapto, and urea groups; X includes at least one of a chloro group, a methoxy group, an ethoxy group, a methoxyethoxy group, and an acetoxy group.