A nitrogen-phosphorus doped ZIF-67 fuel cell catalyst and its preparation method
By using nitrogen and phosphorus doping ZIF-67-derived carbon support and controllable reduction technology, the problem of slow ORR kinetics in fuel cell cathodes was solved, achieving uniform dispersion of platinum particles and stability of the support, reducing platinum usage and preparation costs, making it suitable for commercial applications of fuel cells.
Patent Information
- Application Number
- CN202510868781.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-06-26
AI Technical Summary
The current fuel cell cathode oxygen reduction reaction (ORR) kinetics are slow, and the platinum-based catalyst has low utilization, poor support stability, and insufficient synergistic effect, resulting in rapid degradation of catalyst performance.
A nitrogen-phosphorus-doped ZIF-67-derived carbon support was used to construct a hierarchical porous structure through stepwise doping, and a controllable reduction technique was combined to achieve ultra-dispersed loading of platinum nanoparticles, thereby improving the stability of the support and the dispersibility of platinum particles.
It significantly improves the oxygen reduction reaction rate, extends the catalyst's lifespan, and reduces the amount and cost of platinum used, while also featuring a green and environmentally friendly preparation process.
Smart Images

Figure CN120674518B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fuel cell technology, and in particular to a nitrogen-phosphorus doped ZIF-67 fuel cell catalyst and its preparation method. Background Technology
[0002] In the cathode reaction of fuel cells, the slow kinetics of the oxygen reduction reaction (ORR) is a key factor limiting cell efficiency. Platinum (Pt)-based catalysts are currently the most effective ORR catalysts, but they face three major problems: low platinum utilization: traditional carbon supports (such as Vulcan XC-72) lack active sites on their surface, leading to easy aggregation of Pt nanoparticles (average particle size > 5 nm), with less than 20% of Pt atoms participating in the catalytic reaction; poor support stability: in acidic or alkaline environments, carbon supports are prone to corrosion, causing Pt particles to detach and resulting in rapid degradation of catalyst performance; insufficient synergistic effect: the electronic interaction between a single doped support and Pt is weak, making it difficult to achieve efficient synergistic catalysis of active sites.
[0003] Metal-organic framework (MOF)-derived carbon materials have become a research hotspot due to their high specific surface area and tunable pore structure. ZIF-67, as a cobalt-based MOF, has a certain intrinsic ORR activity in its N-doped carbon framework (Co-N / C) formed after carbonization. However, its ability to regulate the electronic structure of single nitrogen doping is limited, and the introduction of phosphorus is mostly uniform co-doping without gradient distribution design, which means that the dispersion of Pt particles and the stability of the support still need to be improved. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the existing technology and provide a nitrogen-phosphorus doped ZIF-67 fuel cell catalyst and its preparation method. The invention constructs a ZIF-67-derived carbon support with a hierarchical porous structure through stepwise doping and combines it with a controllable reduction technology to achieve ultra-dispersed loading of Pt nanoparticles, thereby improving the dispersibility of Pt particles and the stability of the support.
[0005] The technical solution adopted in this invention is: A nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst, wherein the nitrogen-phosphorus-doped ZIF-67-derived carbon support and platinum nanoparticles supported on the support; the mass fraction of nitrogen doping in the support is 0.5%-2.0%, the mass fraction of phosphorus doping is 1.5%-0.5%, and the loading of platinum nanoparticles is 5%-20%.
[0006] Preferably, the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst has a hierarchical pore structure, including micropores, mesopores, and macropores, wherein the mesopores account for 30%-50%, and the specific surface area of the nitrogen-phosphorus-doped ZIF-67-derived carbon support is ≥1400 m². 2 / g.
[0007] A method for preparing a nitrogen-phosphorus doped ZIF-67 fuel cell catalyst, comprising the following steps: Step S1. Cobalt nitrate and 2-methylimidazole were dissolved in N,N-dimethylformamide and mixed. Then, a microwave-assisted reaction was carried out, followed by centrifugation, washing, and drying to obtain ZIF-67 nanocrystals. Step S2. Disperse ZIF-67 nanocrystals and melamine in an ethanol solution and reflux to allow the melamine to partially embed into the pores. Then, centrifuge, wash, and dry to obtain preliminary nitrogen-doped ZIF-67. Step S3. Disperse the initial nitrogen-doped ZIF-67 with urea and ammonium dihydrogen phosphate in an aqueous solution and stir the reaction. Then centrifuge, wash and dry to obtain the nitrogen-phosphorus-doped ZIF-67 precursor. Step S4. Carbonize the NP-ZIF-67 precursor under an argon atmosphere to obtain a cobalt-containing NG-ZIF-67 precursor. Then, place the carbonized cobalt-containing NG-ZIF-67 precursor in an acid solution and stir to dissolve the cobalt ions in the acid solution. Then, centrifuge, wash, and dry to obtain an NG-ZIF-67 support with metallic cobalt removed. Step S5. Dissolve the NG-ZIF-67 support and the platinum precursor in a solvent according to a Pt loading of 5%-20% and disperse them to obtain a mixture. Then, add NaBH4 aqueous solution dropwise to the mixture. After the addition is complete, stir the reaction. Finally, centrifuge and wash to obtain the Pt-loaded semi-finished product. Step S6. Anneal the Pt-loaded semi-finished product to obtain nitrogen-phosphorus doped ZIF-67 fuel cell catalyst.
[0008] Preferably, in the method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst, the molar ratio of cobalt nitrate and 2-methylimidazole in step S1 is 1:4-1:8, the mixing temperature is 30-50℃, and the time is 1-2h; the microwave-assisted reaction temperature is 120-140℃, and the reaction time is 3-6h.
[0009] Preferably, in the method for preparing the nitrogen-phosphorus doped ZIF-67 fuel cell catalyst, the washing solvent in step S1 is methanol, the number of washing cycles is 3-5, the drying temperature is 60-80℃, and the drying time is 12-24 h.
[0010] Preferably, in the method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst, in step S2, the mass ratio of ZIF-67 nanocrystals to melamine is 1:0.05-1:0.2, the concentration of the ethanol solution is 70-90 vol%, the reflux reaction temperature is 50-70℃, the reflux time is 4-8 h, the washing solvent is ethanol, the washing number is 2-3 times, the drying temperature is 60-80℃, and the drying time is 12-24 h.
[0011] Preferably, in the method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst, in step S3, the mass ratio of the initial nitrogen-doped ZIF-67, urea, and ammonium dihydrogen phosphate is 1:0.1-0.3:0.05-0.2, the stirring reaction temperature is 80-100℃, the time is 6-12 h, the washing solvent is deionized water, the number of washings is 3-5, the drying temperature is 60-80℃, and the drying time is 12-24 h.
[0012] Preferably, in the method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst, the carbonization temperature in step S4 is 700-900℃, the heating rate is 5-10℃ / min, and the carbonization time is 2-4 h; the stirring reaction temperature is 60-80℃, the stirring time is 6-12 h, the drying temperature is 60-80℃, and the drying time is 12-24 h.
[0013] Preferably, in the method for preparing the nitrogen and phosphorus doped ZIF-67 fuel cell catalyst, in step S5, the solvent is ethanol and water with a volume ratio of 2:1-4:1, the dispersion time is 20-40 min, the molar ratio of NaBH4 to Pt is 2-5:1, the stirring temperature is 25-50℃, and the stirring time is 2-4 h.
[0014] Preferably, in the method for preparing the nitrogen-phosphorus doped ZIF-67 fuel cell catalyst, the annealing treatment in step S6 is carried out in a 5% H2 / Ar mixed gas atmosphere, the annealing temperature is 250-350℃, and the annealing time is 1-3h.
[0015] Advantages of this invention: (1) The present invention uses a unique two-step doping method to construct an active site network. In step S2, melamine is initially doped by refluxing at 60°C for 6 hours in an 80 vol% ethanol solution, so that melamine is partially embedded in the ZIF-67 channels to form a basic nitrogen-doped framework. In step S3, urea and ammonium dihydrogen phosphate are stirred in an oil bath at 90°C for 10 hours to achieve secondary nitrogen and phosphorus co-doping. This stepwise strategy can precisely control the doping amount and distribution of nitrogen (0.5%-2.0%) and phosphorus (0.5%-1.5%), forming a cluster of "defect-heteroatom" active sites on the surface and inside the carrier. (2) The phosphorus-doped ZIF-67 fuel cell catalyst of the present invention, from the reaction mechanism perspective, after nitrogen and phosphorus atoms replace carbon atoms in the carbon skeleton, the local electron cloud density is changed, and an electron-rich region is formed on the surface of the support; when platinum nanoparticles are loaded, a strong electronic coupling effect is generated between the support and platinum, the d-band center of platinum shifts, and the adsorption and desorption capacity of O2 and reaction intermediates is optimized. The synergistic effect between the support and platinum significantly reduces the activation energy of the oxygen reduction reaction and improves the reaction rate. (3) The phosphorus-doped ZIF-67 fuel cell catalyst of the present invention has a hierarchical pore structure with transport and stabilization functions. In step S4, cobalt ions are carbonized in an argon atmosphere at 800°C and etched with hydrochloric acid to successfully construct a hierarchical pore structure containing micropores, mesopores (accounting for 30%-50%), and macropores. This structural design improves the catalyst performance in two aspects: Mass transfer optimization: Macropores (>50nm) serve as "high-speed channels" for reactants and products, mesopores (2-50nm) assist in uniform diffusion, and micropores (<2nm) provide high specific surface area for loading active sites; the three work synergistically to significantly reduce mass transfer resistance, enabling O2 and electrolyte to reach the active center quickly. Structural stability: The three-dimensional network of hierarchical channels creates a spatial confinement effect for platinum nanoparticles; during the ORR process, the stress generated by the lattice change of platinum particles can be effectively buffered by the channels, inhibiting particle aggregation and shedding, and the platinum particles of the catalyst are uniformly dispersed in the channels with a particle size of about 2-3 nm; in addition, nitrogen and phosphorus doping further enhances the chemical stability of the support, improves its corrosion resistance, and extends the service life of the catalyst. (4) The phosphorus-doped ZIF-67 fuel cell catalyst of the present invention has a platinum loading optimization and cost reduction mechanism. Based on the excellent performance of the hierarchical pore support, the present invention achieves a significant reduction in platinum loading. In step S5, the platinum loading is controlled at 5%-20% by accurately calculating the amount of platinum salt and ultrasonic dispersion process. Within this loading range, the high specific surface area (≥1400m² / g) and abundant pore structure of the support ensure uniform dispersion of platinum nanoparticles and avoid particle stacking and burying of active sites due to excessive loading. Specifically, the defect sites and heteroatoms formed by nitrogen and phosphorus doping can "anchor" platinum particles on the inner wall of the pores through coordination (such as the lone pair electrons of N and P coordinating with platinum), thereby improving the dispersibility of platinum. Under the same loading, the catalyst of the present invention has a higher catalytic efficiency per unit mass of platinum. When similar ORR performance is achieved, the amount of platinum in the catalyst of the present invention can be reduced by more than 50%, which significantly reduces the cost and provides economic feasibility for the commercialization of fuel cells. (5) The phosphorus-doped ZIF-67 fuel cell catalyst of the present invention adopts multiple green technologies in the preparation process. In terms of solvent system, water / ethanol is used instead of traditional organic solvents (such as N,N-dimethylformamide), which not only reduces the emission of volatile organic compounds, but also allows the ethanol aqueous solution to be recycled and reused, which is in line with the principles of green chemistry. In terms of synthesis process, microwave-assisted synthesis technology is introduced in step S1, which shortens the synthesis time of ZIF-67 nanocrystals from several hours of conventional heating to 4 hours, and the reaction temperature is controlled at 130°C, which significantly reduces energy consumption. Microwave radiation has the characteristics of rapid heating and molecular selective excitation, which makes the reactant molecules vibrate at high frequency, achieving uniform heating and rapid reaction. This technology not only improves the synthesis efficiency, but also promotes the uniform growth of ZIF-67 nanocrystals, laying the foundation for the formation of subsequent hierarchical channels. In addition, no toxic by-products are generated in the preparation process, reducing post-processing costs. It is both environmentally friendly and economical, and is suitable for large-scale industrial production. Attached Figure Description
[0016] Figure 1 is a flowchart of the preparation method of the nitrogen and phosphorus doped ZIF-67 fuel cell catalyst of the present invention.
[0017] Figure 2 is a nitrogen adsorption curve of the NG-ZIF-67 derived carbon support in Example 1 of the present invention.
[0018] Figure 3 is a TEM image of the NG-ZIF-67 derived carbon support of Example 1 of the present invention.
[0019] Figure 4 shows the CV cyclic voltammetry curves of the catalysts prepared in Examples 1-3 and Comparative Example 1 of the present invention.
[0020] Figure 5 shows the ORR polarization curves of the catalysts prepared in Examples 1-3 and Comparative Example 1 of the present invention. Detailed Implementation
[0021] The present invention will be further described below with reference to specific embodiments.
[0022] Example 1 A nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst comprises a nitrogen-phosphorus-doped ZIF-67-derived carbon support and platinum nanoparticles supported on the support; the mass fraction of nitrogen doping in the support is 2.0%, the mass fraction of phosphorus doping is 0.5%, and the loading of platinum nanoparticles is 5%; the nitrogen-phosphorus-doped ZIF-67-derived carbon support has a hierarchical pore structure, including micropores, mesopores, and macropores, wherein mesopores account for 35%, and the specific surface area of the nitrogen-phosphorus-doped ZIF-67-derived carbon support is 1432 m². 2 / g.
[0023] The method for preparing the nitrogen and phosphorus doped ZIF-67 fuel cell catalyst in this embodiment includes the following steps: Step S1. Synthesis of ZIF-67 nanocrystals: 0.01 mol cobalt nitrate and 0.04 mol 2-methylimidazole were dissolved in 50 mL of N,N-dimethylformamide and mixed. The solution was transferred to a three-necked flask and stirred at 200 r / min for 1.5 h in an oil bath at 40 °C. The solution was then transferred to a microwave reactor and microwave-assisted reaction was carried out at 130 °C for 4 h. After the reaction was completed, the product was centrifuged at 4000 r / min for 10 min to obtain a purple precipitate. The precipitate was washed three times with methanol, and centrifuged after each wash. Finally, the washed precipitate was dried at 70 °C for 18 h to obtain ZIF-67 nanocrystals. Step S2. Preliminary nitrogen doping: 1 g of ZIF-67 nanocrystals and 0.1 g of melamine were dispersed in an 80 vol% ethanol solution. The solution was transferred to a round-bottom flask equipped with a condenser and refluxed in a water bath at 60 °C with magnetic stirring at 300 r / min for 6 h to allow the melamine to partially embed into the pores. After the reaction was completed, the solution was centrifuged at 3500 r / min for 8 min. The precipitate was washed twice with ethanol and then dried in a vacuum drying oven at 70 °C for 12 h to obtain preliminary nitrogen-doped ZIF-67. Step S3. Secondary nitrogen and phosphorus doping: 1g of pre-doped nitrogen ZIF-67 was dispersed in an aqueous solution with 0.2g of urea and 0.1g of ammonium dihydrogen phosphate. The mixture was stirred in an oil bath at 90℃ at a stirring speed of 250 r / min for 10h. After that, the mixture was centrifuged at 4500 r / min for 12 min. The precipitate was washed 5 times with deionized water. The washed precipitate was dried in a vacuum drying oven at 70℃ for 24h to obtain the nitrogen and phosphorus doped ZIF-67 precursor. Step S4. Preparation of nitrogen-phosphorus doped carbon support: NP-ZIF-67 precursor was carbonized under an argon atmosphere to obtain cobalt-containing NG-ZIF-67 precursor. The carbonization temperature was 800℃, the heating rate was 5℃ / min, and the carbonization time was 2-3 h. The carbonized cobalt-containing NG-ZIF-67 precursor was then placed in 1M dilute hydrochloric acid and stirred to dissolve cobalt ions in the acid solution. The stirring temperature was 65℃, and the stirring time was 9 h. After centrifugation, the mixture was washed with deionized water until neutral and dried at 70℃ for 20 h to obtain the NG-ZIF-67 support with metallic cobalt removed. The specific surface area of this support was measured to be 1445 m². 2 / g; Step S5. Controllable loading of platinum nanoparticles: Dissolve 0.95 g of NG-ZIF-67 support and 0.133 g of H2PtCl6•6H2O in 60 mL of ethanol and water (volume ratio 3:1) at a Pt loading of 5%. Place the solution in an ultrasonic cleaner and ultrasonically disperse at 100 W for 30 min to obtain a mixture, ensuring thorough wetting of the support pores. Transfer the solution to a three-necked flask and stir at 200 r / min in a 30°C water bath. Then, add 10 mL of 0.1 M NaBH4 aqueous solution (NaBH4:Pt molar ratio 2:1) dropwise at a rate of 1 drop / second. After the addition is complete, stir the mixture at 30°C for 3 h. Centrifuge at 4000 r / min for 10 min, wash the precipitate with deionized water until Cl is undetectable by silver nitrate reagent. - So far, a platinum-loaded semi-finished product has been obtained; Step S6. Place the Pt-loaded semi-finished product into a tube furnace and anneal it in a 5% H2 / Ar mixed gas atmosphere at a temperature of 300℃ for 2 hours. After annealing, allow it to cool naturally to room temperature to obtain the 5% Pt / NG-ZIF-67 catalyst.
[0024] Example 2 The difference between Example 2 and Example 1 is as follows: Step S5. Dissolve 0.9 g of NG-ZIF-67 support and 0.265 g of H2PtCl6•6H2O in 60 mL of ethanol and water with a volume ratio of 3:1, according to a Pt loading of 10%. Place the solution in an ultrasonic cleaner and ultrasonically disperse at 100 W for 30 min to obtain a mixture, ensuring the support pores are fully wetted. Transfer the solution to a three-necked flask and stir at 200 r / min in a 30°C water bath. Then, add 15 mL of 0.1 M NaBH4 aqueous solution (NaBH4:Pt molar ratio of 3:1) dropwise to the mixture at a rate of 1 drop / second. After the addition is complete, stir the reaction mixture at 30°C for 3 h. Centrifuge at 4000 r / min for 10 min, wash the precipitate with deionized water until Cl is undetectable by silver nitrate reagent. - So far, a platinum-loaded semi-finished product has been obtained.
[0025] Step S6. Place the Pt-loaded semi-finished product into a tube furnace and anneal it in a 5% H2 / Ar mixed gas atmosphere at a temperature of 300℃ for 2 hours. After annealing, allow it to cool naturally to room temperature to obtain a 10% Pt / NG-ZIF-67 catalyst.
[0026] Example 3 The difference between Example 3 and Example 1 is as follows: Step S5. Dissolve 0.85 g of NG-ZIF-67 support and 0.398 g of H2PtCl6•6H2O in 60 mL of ethanol and water with a volume ratio of 3:1, according to a Pt loading of 15%. Place the solution in an ultrasonic cleaner and ultrasonically disperse at 120 W for 30 min to obtain a mixture, ensuring the support pores are fully wetted. Transfer the solution to a three-necked flask and stir at 200 r / min in a 40°C water bath. Then, add 20 mL of 0.1 M NaBH4 aqueous solution (NaBH4:Pt molar ratio 4:1) dropwise at a rate of 1 drop / second. After the addition is complete, stir the reaction mixture at 40°C for 3 h. Centrifuge at 4000 r / min for 10 min, wash the precipitate with deionized water until Cl is undetectable by silver nitrate reagent. - So far, a platinum-loaded semi-finished product has been obtained; Step S6. Place the Pt-loaded semi-finished product into a tube furnace and anneal it in a 5% H2 / Ar mixed gas atmosphere at a temperature of 320℃ for 2 hours. After annealing, allow it to cool naturally to room temperature to obtain a 15% Pt / NG-ZIF-67 catalyst.
[0027] Comparative Example 1: 10% Pt / C catalyst (commercial XC-72 support) Comparative Example 1 involves directly loading 10% Pt onto an XC-72 carrier, using the same method as in Example 2.
[0028] The catalysts prepared in Examples 1-3 and Comparative Example 1 were subjected to performance tests.
[0029] Electrochemical performance testing: The oxygen reduction reaction (ORR) performance of the catalyst was tested using rotating disk electrode (RDE) technology in 0.1M HClO4 electrolyte. The test results are shown in Table 1. NG-ZIF-67, as a Pt support, significantly improved the ORR catalytic performance, and the performance showed a linear optimization trend with increasing Pt loading. Compared with the commercial Pt / C in Comparative Example 1, it performed better in terms of activity and Pt utilization efficiency, and is expected to become a candidate support for highly efficient electrochemical catalysts. In Examples 1-3, with the synergistic regulation of nitrogen and phosphorus doping, the half-wave potential of the catalyst gradually increased, indicating a more positive onset potential for the ORR reaction and enhanced catalytic activity. This synergistic effect between the support and platinum significantly reduced the activation energy of the oxygen reduction reaction and increased the reaction rate. Table 1 shows that 10% Pt / NG-ZIF-67... The mass activity (0.103 A / mgPt) is higher than that of commercial 10%Pt / C (0.086 A / mgPt), indicating that the catalyst of the present invention has a higher catalytic efficiency per unit mass of platinum under the same loading. When achieving similar ORR performance, the amount of platinum used in the catalyst of the present invention can be reduced by more than 50%, which significantly reduces the cost and provides economic feasibility for the commercialization of fuel cells.
[0030] Table 1 Catalyst type Half-wave potential (V) Mass activity (A / mgPt) <![CDATA[Electrochemically Active Area (m 2 / g)]]> 5% Pt / NG-ZIF-67 0.925 0.085 66.756 10% Pt / NG-ZIF-67 0.927 0.103 71.415 15% Pt / NG-ZIF-67 0.929 0.146 76.610 10% Pt / C (XC-72) 0.924 0.086 62.175 Figure 2 shows the nitrogen adsorption curve of the NG-ZIF-67 derived carbon support of the present invention, which exhibits typical hierarchical pore structure characteristics. Figure 3 shows the TEM image of the NG-ZIF-67 derived carbon support of the present invention. The TEM image shows that the platinum particles of the catalyst of the present invention are uniformly dispersed in the pores, with a particle size of about 2-3 nm. Figure 4 shows the CV cyclic voltammetry curves of the catalysts prepared in Examples 1-3 and Comparative Example 1 of the present invention. The electrochemical active area of Examples 1-3 is higher than that of the comparative example. Figure 5 shows the ORR polarization curves of the catalysts prepared in Examples 1-3 and Comparative Example 1 of the present invention. The mass activity of 10% Pt / NG-ZIF-67 is higher than that of commercial 10% Pt / C, indicating that under the same loading, the catalyst of the present invention has a higher catalytic efficiency per unit mass of platinum.
[0031] Finally, it should be noted that the above specific embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst, characterized in that, Includes the following steps: Step S1. Cobalt nitrate and 2-methylimidazole are dissolved in N,N-dimethylformamide and mixed. Then, a microwave-assisted reaction is carried out. After centrifugation, washing and drying, ZIF-67 nanocrystals are obtained. Step S2. Disperse ZIF-67 nanocrystals and melamine in an ethanol solution and reflux the reaction to allow the melamine to partially embed into the pores. Then, centrifuge, wash, and dry to obtain preliminary nitrogen-doped ZIF-67. Step S3. Disperse the initial nitrogen-doped ZIF-67 with urea and ammonium dihydrogen phosphate in an aqueous solution and stir the reaction. Then centrifuge, wash and dry to obtain the nitrogen-phosphorus-doped ZIF-67 precursor. Step S4. Carbonize the NP-ZIF-67 precursor under an argon atmosphere to obtain a cobalt-containing NG-ZIF-67 precursor. Then, place the carbonized cobalt-containing NG-ZIF-67 precursor in an acid solution and stir to dissolve the cobalt ions in the acid solution. Then, centrifuge, wash, and dry to obtain an NG-ZIF-67 support with metallic cobalt removed. Step S5. Dissolve the NG-ZIF-67 support and the platinum precursor in a solvent according to the Pt loading of 5%-20% and disperse them to obtain a mixture. Then, add NaBH4 aqueous solution dropwise to the mixture. After the addition is completed, stir the reaction. Finally, centrifuge and wash to obtain the Pt-loaded semi-finished product. Step S6. Anneal the Pt-loaded semi-finished product to obtain a nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst.
2. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, The nitrogen-phosphorus doped ZIF-67 fuel cell catalyst comprises a nitrogen-phosphorus doped ZIF-67 derived carbon support and platinum nanoparticles supported on the support; the mass fraction of nitrogen doping in the support is 0.5%-2.0%, the mass fraction of phosphorus doping is 0.5%-1.5%, and the loading of platinum nanoparticles is 5%-20%.
3. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, Nitrogen-phosphorus doped ZIF-67-derived carbon supports possess a hierarchical pore structure, including micropores, mesopores, and macropores, with mesopores accounting for 30%-50%. The specific surface area of nitrogen-phosphorus doped ZIF-67-derived carbon supports is ≥1400 m². 2 / g.
4. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, In step S1, the molar ratio of cobalt nitrate to 2-methylimidazole is 1:4-1:8, the mixing temperature is 30-50℃, and the time is 1-2h; the microwave-assisted reaction temperature is 120-140℃, and the reaction time is 3-6h.
5. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, In step S1, the washing solvent is methanol, the washing is performed 3-5 times, the drying temperature is 60-80℃, and the drying time is 12-24h.
6. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, In step S2, the mass ratio of ZIF-67 nanocrystals to melamine is 1:0.05-1:0.2, the concentration of the ethanol solution is 70-90 vol%, the reflux reaction temperature is 50-70℃, the reflux time is 4-8 h, the washing solvent is ethanol, the number of washings is 2-3, the drying temperature is 60-80℃, and the drying time is 12-24 h.
7. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, In step S3, the mass ratio of initial nitrogen-doped ZIF-67, urea, and ammonium dihydrogen phosphate is 1:0.1-0.3:0.05-0.
2. The stirring reaction temperature is 80-100℃, the time is 6-12h, the washing solvent is deionized water, the number of washings is 3-5, the drying temperature is 60-80℃, and the drying time is 12-24h.
8. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 3, characterized in that, In step S4, the carbonization temperature is 700-900℃, the heating rate is 5-10℃ / min, and the carbonization time is 2-4h; the stirring reaction temperature is 60-80℃, the stirring time is 6-12h, the drying temperature is 60-80℃, and the drying time is 12-24h.
9. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, In step S5, the solvent is ethanol and water in a volume ratio of 2:1 to 4:1, the dispersion time is 20 to 40 min, the molar ratio of NaBH4 to Pt is 2 to 5:1, the stirring temperature is 25 to 50 °C, and the stirring time is 2 to 4 h.
10. The method for preparing the nitrogen-phosphorus-doped ZIF-67 fuel cell catalyst according to claim 1, characterized in that, In step S6, the annealing process is carried out in a 5% H2 / Ar mixed gas atmosphere, at an annealing temperature of 250-350℃, and for 1-3 hours.
Citation Information
Patent Citations
Preparation method of metal organic framework derived Co embedded nitrogen-doped carbon nanotube modified mesoporous carbon supported platinum catalyst
CN111710878A
Preparation method of nitrogen and phosphorus co-doped platinum carbon catalyst
CN117747859A