Small-grain mordenite molecular sieve as well as preparation method and application thereof

Small-grain MOR molecular sieves were prepared by a segmented crystallization method, which solved the problem of difficult adjustment of grain size and B acid site distribution in the existing technology, achieved efficient catalysis of dimethyl ether carbonylation reaction and catalyst stability, and are suitable for industrial production.

CN120698478APending Publication Date: 2025-09-26DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410345644.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2025-09-26

AI Technical Summary

Technical Problem

It is difficult to adjust the grain size and B acid site distribution of MOR molecular sieves by simply controlling the synthesis process with existing technologies, resulting in limited catalytic performance.

Method used

A segmented controlled crystallization method was adopted to control the morphology and acid distribution of small-grain MOR molecular sieves through two gel mixing and crystallization processes, and a mordenite molecular sieve with a grain diameter of 15nm to 300nm and 8-membered ring channel B acid centers accounting for >70% of the total B acid centers was prepared.

Benefits of technology

The method achieves efficient catalytic carbonylation of dimethyl ether, improves catalytic activity and stability, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120698478A_ABST
    Figure CN120698478A_ABST
Patent Text Reader

Abstract

The invention discloses a small-grain mordenite molecular sieve as well as a preparation method and application thereof, a crystallization process is directionally controlled by adopting a sectional regulation and control crystallization method, so that the morphology and acid distribution of the molecular sieve are regulated and controlled, and the synthesis method is simple in process and suitable for large-scale industrial production; the grain diameter of the small-grain mordenite molecular sieve obtained by the method disclosed by the invention is 15-300nm; the B acid center of the 8-membered ring pore channel accounts for gt of the total B acid center; the catalyst is used for the carbonylation reaction of dimethyl ether, and has good activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to small-grain mordenite molecular sieve and a preparation method and catalytic application thereof, and belongs to the field of inorganic porous materials, adsorption materials and catalytic materials. Background Art

[0002] Mordenite molecular sieve, also known as MOR molecular sieve, is an important class of silica-alumina zeolite molecular sieve materials. As an important adsorption and catalytic material, it is widely used in the fields of petroleum processing, coal chemical industry, and fine chemical industry. The MOR molecular sieve framework consists of parallel 12-membered ring straight channels and 8-membered ring straight channels along the c-axis. Generally speaking, the 8-membered ring channel has a small window size, so it is generally believed that reactants cannot enter the channel through this window. Along the b-axis, there is an 8-membered ring channel connecting the two channels along the c-axis. This 8-membered ring channel has a shorter path and is also called an 8-membered ring side pocket. The acid sites in the different channels of the MOR molecular sieve affect its catalytic application. The acid in the 12-membered ring, due to its larger pore size, can be used as a large-pore molecular sieve to process larger molecules. The acid in the 8-membered ring side pocket, due to its unique confinement effect, has excellent catalytic performance in some small molecule reactions, such as the carbonylation of dimethyl ether to produce methyl acetate. In addition to the acid distribution, the crystal size of the molecular sieve also affects the catalytic performance. Small-crystal molecular sieves are beneficial to improving the accessibility of the active center of the molecular sieve and the reactants. Small-crystal molecular sieves can reduce the diffusion distance between the reactant molecules and the product molecules, which is beneficial to reducing the occurrence of side reactions and improving the life of the catalyst. The prior art generally adjusts the crystal size or acid distribution by changing the template, changing the initial gel composition, etc. Chinese patent CN 108217680A reports a method for synthesizing a MOR molecular sieve with an adjustable octagonal side pocket B acid amount, but the initial gel requires the addition of a fluorination agent and a seed crystal. Wu et al. reported a method for synthesizing mordenite nanosheets of about 10 nm (Angew. Chem. Int. Ed. 2020, 59, 6258-6262), but it is necessary to use a cationic gemini surfactant with a complex structure. Directly preparing MOR molecular sieves with adjustable B acid site distribution and crystal size by simply controlling the synthesis process rather than the raw material composition still faces huge challenges. Summary of the Invention

[0003] The present invention provides a small-grain MOR molecular sieve and a preparation method and application thereof. The small-grain MOR molecular sieve can efficiently catalyze the carbonylation reaction of dimethyl ether.

[0004] According to the first aspect of the present application, a small-grain mordenite molecular sieve is provided, which is composed of grains with a grain diameter of 15nm to 300nm; in the small-grain mordenite molecular sieve, the Br acid centers of the 8-membered ring channels account for >70% of the total Br acid centers.

[0005] Optionally, the crystal particles have a granular or columnar crystal morphology; preferably, the small-crystal mordenite molecular sieve has a block-like morphology macroscopically.

[0006] Optionally, in the small-grain mordenite molecular sieve, the acid centers of the 8-membered ring channels account for 70-95% of the total B acid centers.

[0007] Optionally, the silicon-aluminum molecular sieve in the small-grain mordenite molecular sieve has a molar ratio of 15 to 250.

[0008] The second aspect of the present application provides a method for preparing the small-grain mordenite molecular sieve according to the first aspect of the present application, comprising the following steps:

[0009] (1) providing a first gel mixture, comprising a first silicon source, a first aluminum source, a first template, water, and a first alkali source; the first silicon source is calculated as SiO2, the first aluminum source is calculated as Al2O3, and the first alkali source is calculated as R2O; and in the first gel mixture, the molar ratio of the first silicon source, the first aluminum source, the first template, water, and the first alkali source is A1:B1:C1:D1:E1=1:0.01-0.2:0-0.5:5-35:0-0.5;

[0010] (2) crystallizing the first gel mixture;

[0011] (3) providing a second gel mixture, which comprises a second silicon source, a second aluminum source, a second template, water, and a second alkali source; the second silicon source is calculated as SiO2, the second aluminum source is calculated as Al2O3, and the second alkali source is calculated as R2O, and the molar ratio of the second silicon source to the second silicon source, the second aluminum source, the second template, water, and the second alkali metal hydroxide in the second gel compound is A1:A2:B2:C2:D2:E2=1:0-3:0-0.2:0-0.5:0-35:0-0.5 based on the first silicon source;

[0012] And C1+C2>0; E1+E2>0; A2+B2+C2+E2>0;

[0013] mixing the slurry obtained in step (2) with the second gel mixture;

[0014] (4) crystallizing the mixture of step (3);

[0015] (5) separating the solid product obtained in step (4), washing it to neutrality, and drying it to obtain small-grain mordenite molecular sieve raw powder;

[0016] (6) calcining the raw powder of the small-crystal mordenite molecular sieve, removing inorganic alkali metal ions by ion exchange, and then calcining to obtain the small-crystal mordenite molecular sieve.

[0017] Optionally, in step (1), the molar ratio of the first silicon source, the first aluminum source, the first template, water and the first alkali source is 1:0.01-0.067:0-0.3:8-35:0-0.3;

[0018] Preferably, in step (3), the molar ratio of the first silicon source, the second silicon source, the second aluminum source, the second template, water and the second alkali source is 1:0-3:0-0.067:0-0.33:5-35:0-0.3.

[0019] Optionally, the first silicon source and the second silicon source are each independently selected from one or more of coarse-pore silicon powder, fine-pore silicon powder, silica sol, ethyl orthosilicate, white carbon black and water glass;

[0020] Preferably, the first aluminum source and the second aluminum source are independently selected from one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, sodium metaaluminate, aluminum sol, aluminum isopropoxide, and aluminum isobutoxide.

[0021] Optionally, the first template and the second template are each independently selected from one or more of methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, N-methyldiethylamine, N,N-dimethylethylamine, N-methylethylenediamine, N,N-dimethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N-diethylethylenediamine, N,N,N'-triethylethylenediamine, n-propylamine, di-n-propylamine, isopropylamine, tetramethylammonium hydroxide, tetramethylammonium bromide, tetramethylammonium chloride, tetramethylammonium iodide, tetraethylammonium hydroxide, tetraethylammonium bromide, tetraethylammonium chloride, tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrapropylammonium chloride, methanol, ethanol, n-propanol and isopropanol.

[0022] Optionally, the first alkali source and the second alkali source are each independently selected from one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide.

[0023] Optionally, the crystallization conditions in step (2) and step (4) are independently selected from a crystallization temperature of 150 to 220° C. and crystallization under autogenous pressure for 5 to 100 hours;

[0024] Optionally, the crystallization states in step (2) and step (4) are each independently selected from dynamic crystallization or static crystallization.

[0025] The third aspect of the present application provides a small-grain mordenite molecular sieve catalyst, comprising the small-grain mordenite molecular sieve provided by the first aspect of the present application or the small-grain mordenite molecular sieve prepared by the method provided by the second aspect of the present application and a binder.

[0026] The third aspect of the present application provides a method for preparing methyl acetate by carbonylation of dimethyl ether, comprising the step of subjecting dimethyl ether to a carbonylation reaction in the presence of a catalyst, wherein the catalyst is the small-grain mordenite molecular sieve provided by the first aspect of the present application, or the small-grain mordenite molecular sieve prepared by the method provided by the second aspect of the present application, or the molecular sieve catalyst provided by the third aspect of the present application.

[0027] The beneficial effects of this application include:

[0028] (1) The present invention adopts a segmented crystallization method to control the crystallization process in a directionally controlled manner, thereby regulating the morphology and acid distribution of the molecular sieve.

[0029] (2) The MOR molecular sieve of small crystal grains synthesized by the present invention has a crystal diameter of 15 nm to 300 nm and an eight-membered cyclic acid distribution of more than 70%.

[0030] (3) The MOR molecular sieve synthesized in the present invention is used for dimethyl ether carbonylation reaction and has good activity and stability.

[0031] (4) The synthesis method of the present invention is simple and suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 XRD analysis spectrum of the small-grain mordenite molecular sieve raw powder synthesized in Example 1.

[0033] Figure 2 SEM analysis photograph of the small-grain mordenite molecular sieve raw powder synthesized in Example 1.

[0034] Figure 3 FT-IR analysis spectrum of the small-grain mordenite molecular sieve synthesized in Example 1.

[0035] Figure 4 SEM photograph of the product synthesized in Example 3.

[0036] Figure 5 SEM photograph of the product synthesized in Example 6.

[0037] Figure 6 SEM photograph of the product synthesized in Example 8. DETAILED DESCRIPTION

[0038] The first aspect of the present application provides a small-grain mordenite molecular sieve, which is composed of grains, and the grain diameter of the grains is 15nm to 300nm; in the small-grain mordenite molecular sieve, the Br acid centers in the eight-membered ring "side pockets" account for >70% of the total Br acid centers.

[0039] In this application, "B acid" has its general meaning in this field, and mainly refers to the acidic hydroxyl groups carried by the aluminum oxide tetrahedron on the framework of the zeolite crystal.

[0040] In this application, the Br acid centers in the eight-membered ring "side pocket" account for >70% of the total Br acid centers and thus have higher catalytic activity.

[0041] In some embodiments, the grains have a granular or columnar crystal morphology.

[0042] In some embodiments, the small-crystal mordenite molecular sieve has a block-like morphology in macroscopic terms.

[0043] In some embodiments, in the small-grain mordenite molecular sieve, the acid centers of the 8-membered ring channels account for 70-95% of the total B acid centers.

[0044] Optionally, the silicon-aluminum molecular sieve in the small-grain mordenite molecular sieve has a molar ratio of 15 to 250.

[0045] The second aspect of the present application provides a method for preparing the small-grain mordenite molecular sieve according to the first aspect of the present application, comprising the following steps:

[0046] (1) providing a first gel mixture, comprising a first silicon source, a first aluminum source, a first template, water, and a first alkali source; the first silicon source is calculated as SiO2, the first aluminum source is calculated as Al2O3, and the first alkali source is calculated as R2O; and in the first gel mixture, the molar ratio of the first silicon source, the first aluminum source, the first template, water, and the first alkali source is A1:B1:C1:D1:E1=1:0.01-0.2:0-0.5:5-35:0-0.5;

[0047] (2) crystallizing the first gel mixture;

[0048] (3) providing a second gel mixture, which comprises a second silicon source, a second aluminum source, a second template, water, and a second alkali source; the second silicon source is calculated as SiO2, the second aluminum source is calculated as Al2O3, and the second alkali source is calculated as R2O, and the molar ratio of the second silicon source to the second silicon source, the second aluminum source, the second template, water, and the second alkali metal hydroxide in the second gel compound is A1:A2:B2:C2:D2:E2=1:0-3:0-0.2:0-0.5:0-35:0-0.5 based on the first silicon source;

[0049] And C1+C2>0; E1+E2>0; A2+B2+C2+E2>0;

[0050] mixing the slurry obtained in step (2) with the second gel mixture;

[0051] (4) crystallizing the mixture of step (3);

[0052] (5) separating the solid product obtained in step (4), washing it to neutrality, and drying it to obtain small-grain mordenite molecular sieve raw powder;

[0053] (6) calcining the raw powder of the small-crystal mordenite molecular sieve, removing inorganic alkali metal ions by ion exchange, and then calcining to obtain the small-crystal mordenite molecular sieve.

[0054] The method of the present application changes the crystallization direction of the grains in the molecular sieve through the second crystallization, thereby regulating the distribution of B acid and the grain size.

[0055] The method of the present application can use conventional raw materials for preparing mordenite molecular sieves, without adding components such as fluorination agents and seed crystals for controlling crystallization, thereby achieving regulation of B acid site distribution and grain size by controlling the synthesis process.

[0056] In the preparation method of the present application, conventional raw materials for preparing mordenite molecular sieves can be used: silicon source, aluminum source, template agent, water and alkali source.

[0057] In some embodiments, these five raw materials can exist simultaneously in the first gel compound and complete the first crystallization. At this time, any one of the four raw materials except water can be selected from the second gel compound, with or without water, as the second gel compound, added to the slurry obtained by crystallizing the first gel mixture, and subjected to a second crystallization.

[0058] In other embodiments, the first gel compound may contain at least a silicon source, an aluminum source and water, and optionally may also contain at least one of a template agent and an alkali source, and complete the first crystallization; at this time, the second gel compound must contain at least raw materials not contained in the first gel compound, and optionally may also contain raw materials already contained in the first gel, and undergo a second crystallization.

[0059] In some specific embodiments, the first gel compound comprises a first silicon source, a first aluminum source, and water; the second gel compound comprises a template agent and an alkali source, and optionally further comprises a second silicon source, a second aluminum source, and / or water.

[0060] In some specific embodiments, the first gel compound comprises a first silicon source, a first aluminum source, a first template agent, and water; the second gel compound comprises an alkali source and, optionally, a second silicon source, a second template agent, a second aluminum source, and / or water. In this embodiment, the alkali source and the template agent can be interchangeable.

[0061] In some specific embodiments, the first gel compound comprises a first silicon source, a first aluminum source, a first template agent, a first alkali source and water; the second gel compound comprises at least one of a second silicon source, a second aluminum source, a second template agent, a second alkali source and optionally water.

[0062] In some embodiments, in step (1), the molar ratio of the first silicon source, the first aluminum source, the first template, water and the first alkali source is 1:0.01-0.067:0-0.3:8-35:0-0.3.

[0063] In some embodiments, in step (3), the molar ratio of the first silicon source, the second silicon source, the second aluminum source, the second template, water, and the second alkali source is 1:0-3:0-0.067:0-0.33:5-35:0-0.3.

[0064] In some embodiments, the first silicon source and the second silicon source are each independently selected from one or more of coarse-pore silicon powder, fine-pore silicon powder, silica sol, tetraethyl orthosilicate, white carbon black, and water glass.

[0065] In some embodiments, the first silicon source and the second silicon source may be selected the same or different.

[0066] In some embodiments, the first aluminum source and the second aluminum source are each independently selected from one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, sodium metaaluminate, aluminum sol, aluminum isopropoxide, and aluminum isobutoxide.

[0067] In some embodiments, the selection of the first aluminum source and the second aluminum source can be the same or different.

[0068] In some embodiments, the first templating agent and the second templating agent are each independently selected from one or more of methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, N-methyldiethylamine, N,N-dimethylethylamine, N-methylethylenediamine, N,N-dimethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N-diethylethylenediamine, N,N,N'-triethylethylenediamine, n-propylamine, di-n-propylamine, isopropylamine, tetramethylammonium hydroxide, tetramethylammonium bromide, tetramethylammonium chloride, tetramethylammonium iodide, tetraethylammonium hydroxide, tetraethylammonium bromide, tetraethylammonium chloride, tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrapropylammonium chloride, methanol, ethanol, n-propanol and isopropanol.

[0069] In some embodiments, the first templating agent and the second templating agent may be selected to be the same or different.

[0070] In some embodiments, the first alkaline source and the second alkaline source are each independently selected from one or more of lithium hydroxide, sodium hydroxide, and potassium hydroxide.

[0071] In some embodiments, the first alkaline source and the second alkaline source may be selected the same or different.

[0072] In some embodiments, the crystallization conditions in step (2) and step (4) are independently selected from a crystallization temperature of 150 to 220° C. and crystallization under autogenous pressure for 5 to 100 hours.

[0073] In some embodiments, the crystallization states in step (2) and step (4) are each independently selected from dynamic crystallization or static crystallization.

[0074] In some embodiments, the crystallization conditions in step (2) and step (4) may be the same or different.

[0075] In some embodiments, the solid product obtained in step (4) can be isolated by filtration.

[0076] In some embodiments, the solid product can be washed by conventional means, such as washing with deionized water until neutral. The washing method is a conventional technical means in the art and is not limited in this application.

[0077] In some embodiments, in step (6), conventional calcination can be used before the ion exchange method is used to remove the inorganic alkali metal ions, for example, calcination at 500-600°C in air for 3-5 hours, the purpose of which is to remove the template agent. Those skilled in the art are capable of selecting conventional calcination conditions based on the selection and dosage of the template agent, and this application does not limit this.

[0078] In some embodiments, in step (6), the calcination after removing the inorganic alkali metal ions by ion exchange can be conventional calcination, for example, calcination in air at 500-600°C for 3-5h, the purpose of which is to obtain a hydrogen-type molecular sieve. This is a conventional operation in the art and is not limited in this application.

[0079] The third aspect of the present application provides a small-grain mordenite molecular sieve catalyst, comprising the small-grain mordenite molecular sieve provided by the first aspect of the present application or the small-grain mordenite molecular sieve prepared by the method provided by the second aspect of the present application, and a binder.

[0080] The third aspect of the present application provides a method for preparing methyl acetate by carbonylation of dimethyl ether, comprising the step of subjecting dimethyl ether to a carbonylation reaction in the presence of a catalyst, wherein the catalyst is the small-grain mordenite molecular sieve provided by the first aspect of the present application, or the small-grain mordenite molecular sieve prepared by the method provided by the second aspect of the present application, or the molecular sieve catalyst provided by the third aspect of the present application.

[0081] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0082] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0083] The analysis method in the examples of this application is as follows:

[0084] X-ray powder diffraction (XRD) phase analysis was performed using an X'Pert PRO X-ray diffractometer from PANalytical, the Netherlands, with a Cu target, a Kα radiation source (λ=0.15418 nm), a voltage of 40 kV, and a current of 40 mA.

[0085] The scanning electron microscope (SEM) test instrument used was a Hitachi SU8020 field emission scanning electron microscope with an accelerating voltage of 2 kV.

[0086] The infrared transmission spectroscopy (FTIR) experiment was carried out in a vacuum system. The samples were dehydrated at 450 °C and the spectra were collected at room temperature.

[0087] X-ray fluorescence (XRF) analysis was performed using a Philips Magix-601 X-ray fluorescence spectrometer. Molecular sieve samples were pressed into pellets at 30 MPa prior to analysis. Test conditions: voltage 40 kV, current 40 mA.

[0088] Gas sample analysis was performed on-line using an Agilent 6890GC gas chromatograph, and the chromatographic column was an Agilent HP-5 capillary column.

[0089] Unless otherwise specified, the raw materials and catalysts in the examples of this application were purchased from commercial channels and used directly without any special treatment.

[0090] In the examples, the conversion of dimethyl ether and the selectivity of methyl acetate are calculated based on the carbon moles of dimethyl ether:

[0091] Dimethyl ether conversion rate = [(mole number of dimethyl ether carbon in the feed gas) - (mole number of dimethyl ether carbon in the product)] ÷ (mole number of dimethyl ether carbon in the feed gas) × (100%)

[0092] Methyl acetate selectivity = (2 / 3) × (mole number of carbon atoms of methyl acetate in the product) ÷ [(mole number of carbon atoms of dimethyl ether in the feed gas) – (mole number of carbon atoms of dimethyl ether in the product)] × (100%)

[0093] Example 1

[0094] The molar ratios of the raw materials in the gel and the crystallization conditions are shown in Table 1. Gel 1: Dissolve 1.77g of solid sodium hydroxide, 2.83g of sodium metaaluminate, and 5.05g of triethylamine in 68.90g of deionized water. After mixing, add 16.30g of white carbon black and stir until uniform. This is designated as 1#-1. Gel 2: Dissolve 1.77g of solid sodium hydroxide, 2.83g of sodium metaaluminate, and 5.05g of triethylamine in 68.90g of deionized water. After mixing, add 16.30g of white carbon black and stir until uniform. This is designated as 1#-2. Gel 1 was placed in a stainless steel reactor with a polytetrafluoroethylene lining and heated to 160°C for crystallization for 18 hours. Gel 2 was then added to the reactor and crystallized at 160°C for 39 hours. The resulting solid product was centrifuged, washed with deionized water until neutral, and air-dried at 110°C to obtain the original powder, designated as Sample 1#.

[0095] The obtained sample 1# was subjected to XRD analysis, and the results showed that the synthesized product had the characteristics of MOR structure. Figure 1 The sample morphology was analyzed by SEM, and it was found that the molecular sieve was in the form of particles of about 20 nm. Figure 2 As shown. The sample composition was analyzed by XRF, and the results are listed in Table 2. The silicon-aluminum ratio (SiO2 / Al2O3) of the sample in Example 1 is 25.5. The original molecular sieve powder was calcined in air at 550°C for 4 hours to remove the template, and then the calcined sample was placed in a beaker, and 1 mol / L ammonium nitrate solution was added to the beaker and exchanged at 80°C for 2 hours. After repeating the exchange three times, it was dried at 120°C for 8 hours and then calcined in air at 550°C for 4 hours to obtain a hydrogen-type molecular sieve, that is, the small-grained silk zeolite molecular sieve of the present application. The hydrogen-type molecular sieve was subjected to FT-IR detection, and the 3605 cm -1 The peak fitting is performed on the nearby bridge hydroxyl groups, and the results are as follows Figure 3 The results show that the percentage of 8-membered ring channel Br acid in the sample accounts for 73% of the total Br acid.

[0096] Examples 2-14

[0097] The specific proportions of ingredients and crystallization conditions are shown in Table 1, and the specific preparation process is the same as in Example 1.

[0098] The synthesized samples 2#-14# were subjected to XRD analysis, and the data results were consistent with Figure 1 The diffraction peak positions and shapes are similar, and the relative peak intensity fluctuates within the range of ±5% depending on the synthesis conditions, indicating that the synthesized product has pure phase MOR.

[0099] Referring to Example 1, the grain size obtained by SEM analysis and the silicon-aluminum ratio obtained by XRF analysis of the samples synthesized in each example are listed in Table 2. Among them, the SEM results of Example 3 are as follows: Figure 4 As shown, the SEM results of Example 6 are as follows Figure 5 As shown, the SEM results of Example 8 are as follows Figure 6 According to the method in Example 1, samples 2#-14# were converted into hydrogen forms through ammonium exchange and then subjected to FT-IR analysis. The analysis method was the same as in Example 1. The test results of the 8-membered ring B acid ratio of the samples are listed in Table 2.

[0100] Comparative Example 1

[0101] The solid product of gel 1 in Example 1 after crystallization was directly centrifuged, washed with deionized water until neutral, and dried in air at 110° C. to obtain raw powder, which was recorded as sample 13#.

[0102] The synthesized sample 13# was subjected to XRD analysis, and the data results were consistent with Figure 1 The diffraction peak positions and shapes are similar, and the relative peak intensity fluctuates within the range of ±5% depending on the synthesis conditions, indicating that the synthesized product has pure phase MOR.

[0103] The synthesized samples were subjected to SEM analysis, and the SEM results are shown in Table 2, indicating that the MOR is composed of grains; XRF analysis shows that the molecular sieve silicon-aluminum ratio results are shown in Table 2; according to the method in Example 1, sample 13# was converted into a hydrogen form through ammonium exchange, and then subjected to FT-IR testing. The analysis method was the same as in Example 1, and the test results are listed in Table 2.

[0104] Table 1 Molar ratio of each raw material and crystallization conditions in the gel of Example 1-Example 14

[0105]

[0106]

[0107] a. Ethyl orthosilicate, b. White carbon black, c. Silica sol, d. Coarse-porous silica powder, e. Sodium metaaluminate, f. Aluminum nitrate, g. Triethylamine, h. Tetraethylammonium hydroxide, i. Tetramethylammonium hydroxide, j. Sodium hydroxide, k. Potassium hydroxide

[0108] The proportions of each component are based on the first silicon source in each embodiment.

[0109] Table 2 Test results of samples synthesized in Examples 1 to 14 and Comparative Example 1

[0110]

[0111]

[0112] Test Example 1

[0113] 1.0 g of the hydrogen-type molecular sieve obtained in Example 1 was weighed and evaluated for dimethyl ether carbonylation in a fixed-bed reactor. The reaction was initially activated with nitrogen at 400°C for 1 hour, then cooled to 300°C. Pyridine was introduced into the reactor at a gas flow rate of 30 ml / min for 1 hour, followed by a nitrogen purge for 1 hour. Finally, the temperature was lowered to 200°C for reaction. The gas mixture was (DME / CO / N2 = 5 / 30 / 65, volume ratio), with a gas flow rate of 200 ml / min and a reaction pressure of 2 MPa. The results after different reaction times are listed in Table 3.

[0114] Test Example 2-5

[0115] Except for the different molecular sieve samples, the other reaction conditions were the same as those in Test Example 1. The specific reaction time and reaction results are shown in Table 3.

[0116] Table 3 Reaction results of samples of Examples 13-18

[0117]

[0118]

[0119] As can be seen from the results in Table 3, the small-grain mordenite molecular sieve of the present application can achieve a higher dimethyl ether conversion rate when catalyzing the carbonylation of dimethyl ether to produce methyl acetate, wherein the dimethyl ether conversion rate increases with an increase in the proportion of 8-membered ring B acid in the molecular sieve; and the molecular sieve of the present application can still maintain a high catalytic activity after 8000 hours of operation, indicating that the catalyst of the present application has higher stability and catalytic activity.

[0120] The above descriptions are merely a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application discloses the preferred embodiments as above, they are not intended to limit the present application. Any technical personnel familiar with the present profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A small-grain mordenite molecular sieve, characterized in that: The small-crystal mordenite molecular sieve is composed of crystal grains, the crystal grains have a diameter of 15nm to 300nm; in the small-crystal mordenite molecular sieve, the Br acid centers of the 8-membered ring channels account for more than 70% of the total Br acid centers.

2. The molecular sieve according to claim 1, characterized in that The crystal particles have a granular or columnar crystal morphology; preferably, the small-crystal mordenite molecular sieve has a block-like morphology macroscopically.

3. The molecular sieve according to claim 1, characterized in that In the small-crystal mordenite molecular sieve, the acid centers of the 8-membered ring channels account for 70-95% of the total B acid centers.

4. The molecular sieve according to claim 1, characterized in that The silicon and aluminum molecular moles in the small-grain mordenite molecular sieve are 15-250.

5. The method for preparing small-grain mordenite molecular sieve according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) providing a first gel mixture, comprising a first silicon source, a first aluminum source, a first template, water, and a first alkali source; the first silicon source is calculated as SiO2, the first aluminum source is calculated as Al2O3, and the first alkali source is calculated as R2O; and in the first gel mixture, the molar ratio of the first silicon source, the first aluminum source, the first template, water, and the first alkali source is A1:B1:C1:D1:E1=1:0.01-0.2:0-0.5:5-35:0-0.5; (2) crystallizing the first gel mixture; (3) providing a second gel mixture, which comprises a second silicon source, a second aluminum source, a second template, water, and a second alkali source; the second silicon source is calculated as SiO2, the second aluminum source is calculated as Al2O3, and the second alkali source is calculated as R2O, and the molar ratio of the second silicon source to the second silicon source, the second aluminum source, the second template, water, and the second alkali metal hydroxide in the second gel compound is A1:A2:B2:C2:D2:E2=1:0-3:0-0.2:0-0.5:0-35:0-0.5 based on the first silicon source; And C1+C2>0; E1+E2>0; A2+B2+C2+E2>0; mixing the slurry obtained in step (2) with the second gel mixture; (4) crystallizing the mixture of step (3); (5) separating the solid product obtained in step (4), washing it to neutrality, and drying it to obtain small-grain mordenite molecular sieve raw powder; (6) calcining the raw powder of the small-crystal mordenite molecular sieve, removing inorganic alkali metal ions by ion exchange, and then calcining to obtain the small-crystal mordenite molecular sieve.

6. The preparation method according to claim 5, characterized in that In the step (1), the molar ratio of the first silicon source, the first aluminum source, the first template, water and the first alkali source is 1:0.01-0.067:0-0.3:8-35:0-0.3; Preferably, in step (3), the molar ratio of the first silicon source, the second silicon source, the second aluminum source, the second template, water and the second alkali source is 1:0-3:0-0.067:0-0.33:5-35:0-0.

3.

7. The preparation method according to claim 5, characterized in that The first silicon source and the second silicon source are each independently selected from one or more of coarse-pore silicon powder, fine-pore silicon powder, silica sol, ethyl orthosilicate, white carbon black and water glass; Preferably, the first aluminum source and the second aluminum source are each independently selected from one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, sodium metaaluminate, aluminum sol, aluminum isopropoxide, and aluminum isobutoxide; Preferably, the first template and the second template are each independently selected from one or more of methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, N-methyldiethylamine, N,N-dimethylethylamine, N-methylethylenediamine, N,N-dimethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N-diethylethylenediamine, N,N,N'-triethylethylenediamine, n-propylamine, di-n-propylamine, isopropylamine, tetramethylammonium hydroxide, tetramethylammonium bromide, tetramethylammonium chloride, tetramethylammonium iodide, tetraethylammonium hydroxide, tetraethylammonium bromide, tetraethylammonium chloride, tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrapropylammonium chloride, methanol, ethanol, n-propanol and isopropanol; Preferably, the first alkali source and the second alkali source are each independently selected from one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide.

8. The preparation method according to claim 5, characterized in that The crystallization conditions in step (2) and step (4) are independently selected from the crystallization temperature of 150 to 220° C. and crystallization under autogenous pressure for 5 to 100 hours; Preferably, the crystallization states in step (2) and step (4) are each independently selected from dynamic crystallization or static crystallization.

9. A small-grain mordenite molecular sieve catalyst, characterized in that: The invention comprises the small-crystal mordenite molecular sieve according to any one of claims 1 to 4 or the small-crystal mordenite molecular sieve prepared by the method according to any one of claims 5 to 8 and a binder.

10. A method for preparing methyl acetate by carbonylation of dimethyl ether, characterized in that: The method comprises the step of subjecting dimethyl ether to carbonylation in the presence of a catalyst, wherein the catalyst comprises the small-crystal mordenite molecular sieve according to any one of claims 1 to 4, the small-crystal mordenite molecular sieve prepared by the method according to any one of claims 5 to 8, or the molecular sieve catalyst according to claim 9.

Citation Information

Patent Citations

  • Method for synthesizing mordenite (MOR) molecular sieve as well as product and application of molecular sieve

    CN108217680A

Cited By

  • Mordenite molecular sieve as well as preparation method and application thereof

    CN121778748A