All-solid waste aggregate grouting body and preparation method thereof

By using all-solid waste aggregate grouting bodies, the problem of insufficient strength and stability of grouting bodies in desert environments is solved, the preparation of high-strength and stable grouting bodies is achieved, carbon emissions are reduced, and industrial waste is utilized as a resource, which is suitable for engineering needs in desert areas.

CN120698753AActive Publication Date: 2025-09-26INNER MONGOLIA UNIV OF TECH +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202511225124.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-29
Publication Date
2025-09-26
Estimated Expiration
2045-08-29

AI Technical Summary

Technical Problem

The existing grouting bodies have difficulty adapting to the strength and stability of desert environments, and cement production has high carbon emissions, leading to environmental pollution and waste of resources.

Method used

A grouting body made of all-solid waste aggregate, including pre-treated coal gangue, modified carbide slag, blast furnace slag and ultra-fine fly ash as the base materials, is prepared in combination with composite additives to produce a grouting body with high fluidity and strength. The desert sand is modified to enhance the adhesion and stability.

Benefits of technology

It achieves high strength and stability of the grouting body in desert environments, reduces carbon emissions, and utilizes industrial waste as a resource, making it suitable for reinforcement and repair projects in desert areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120698753A_ABST
    Figure CN120698753A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of all-solid waste grouting bodies, in particular to an all-solid waste aggregate grouting body and a preparation method thereof. The all-solid waste aggregate grouting body comprises a slurry body and pretreated desert sand. Wherein the slurry comprises a base material, a composite additive and water. The base material comprises the following components in parts by mass: 25-40 parts of pretreated coal gangue, 15-25 parts of modified carbide slag, 25-35 parts of blast furnace slag and 10-25 parts of superfine fly ash; the mass of the composite additive is 5-12% of the mass of the base material, and the composite additive is prepared from hydrogenated cocinic acid, glucosylrutin and ethylene-vinyl acetate copolymer emulsion according to the mass ratio of (2-3): 3: 4; the mass ratio of the water to the base material is (0.3-0.35): 1; the mass of the pretreated desert sand is 40% of that of the slurry. According to the all-solid waste aggregate grouting body and the preparation method thereof, the problem that the strength and stability of a grouting body in the related technology are difficult to adapt to the desert environment is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of all-solid waste grouting bodies, and in particular to an all-solid waste aggregate grouting body and a preparation method thereof. Background Art

[0002] With the rapid development of industrialization, the production of bulk industrial solid waste is showing a rapid growth trend, and industrial waste has become a topic of increasing social concern. Industrial waste not only occupies a large amount of land, but also wastes manpower and material resources. Industrial waste contains a large amount of water-soluble substances, causing pollution to the land, groundwater, and air environment. For example, solid wastes such as coal gangue, calcium carbide slag, and blast furnace slag can be used to prepare all-solid waste aggregate grouting materials, which can help realize the resource utilization and high-value utilization of industrial solid waste.

[0003] Current grouting materials are composed of cement and other components. The cement industry is a major energy consumer and carbon emitter. From a process perspective, the production of one ton of Portland cement clinker emits approximately 0.488 to 0.583 tons of carbon dioxide. Cement production relies on coal as a fuel, and the combustion process produces approximately 0.290 to 0.317 tons of carbon dioxide per ton of cement. Calculations show that total carbon dioxide emissions per ton of cement clinker are approximately 0.813 to 0.942 tons. As of 2020, the cement industry's carbon emissions were approximately 13.7 tons, accounting for approximately 13% of China's total carbon emissions and 84.3% of the building materials industry's total carbon emissions.

[0004] Deserts account for more than one-third of the world's land area. The geological conditions in desert areas are complex. The geology of desert areas is usually composed of aeolian sand. This type of soil has poor stability and insufficient adhesion. It is prone to collapse during the drilling process, making it difficult to drill holes and impossible to drive bored piles. Therefore, in desert areas, grouting is usually chosen to meet the purpose of steel pipe piles' compression and pull-out resistance.

[0005] The grouting material needs to be able to pass smoothly through the delivery pipeline and fill the gaps around the steel pipes, so it needs to have good fluidity and permeability. At the same time, to ensure the stability of the steel pipe piles, the grouting material needs to have high strength to withstand the load of the steel pipe piles and the pressure of the surrounding soil. In addition, in the high temperature and windy sand environment of the desert, the grouting material also needs to have good volume stability and be less likely to shrink or crack. The desert climate is harsh, with strong winds and sand and large temperature fluctuations, which places high demands on the durability of the grouting material. Summary of the Invention

[0006] The present application provides a full-solid waste aggregate grouting body and a preparation method thereof, in order to solve the problem in the related art that the strength and stability of the grouting body are difficult to adapt to the desert environment.

[0007] In a first aspect, a full solid waste aggregate grouting body is provided, which includes a slurry and pretreated desert sand: The slurry includes a base material, a composite additive and water; According to the weight ratio, the base material includes 25-40 parts of pretreated coal gangue, 15-25 parts of modified carbide slag, 25-35 parts of blast furnace slag, and 10-25 parts of ultrafine fly ash; The mass of the composite additive is 5-12% of the mass of the base material, and the composite additive includes hydrogenated coconut oil, glucosylrutin and ethylene-vinyl acetate copolymer emulsion in a mass ratio of (2-3):3:4; The ratio of the mass of the water to the mass of the base material is (0.3-0.35):1; The mass of the pretreated desert sand is 40% of the slurry.

[0008] Preferably, the method for preparing pretreated desert sand comprises the following steps: After passing the desert sand through a 30-mesh sieve, the sand was soaked in a 0.1 mol / L oxalic acid solution for 1.5 to 2 h, rinsed with clean water until neutral, and dried at 100 to 105°C to obtain pretreated desert sand.

[0009] Preferably, the preparation of the pretreated gangue comprises the following steps: The gangue and the modifying liquid were mixed in a mass ratio of 1:(0.1-0.25), stirred in an 80°C water bath for 55-60 minutes, and then allowed to stand for 24 hours to obtain pretreated gangue; The modified liquid comprises wood vinegar, conchiolin powder and water in a mass ratio of 3:(2-3):100.

[0010] Preferably, the particle size of the coal gangue is 3-4.5 cm.

[0011] Preferably, the preparation method of the modified carbide slag is as follows: passing the carbide slag through a 200-mesh sieve, then placing the sieved carbide slag into a muffle furnace for calcination, heating the temperature to 750-760° C. at a rate of 20° C. / min, and calcining at 750-760° C. for 1-2.5 hours. After the calcination is completed, the carbide slag is taken out of the muffle furnace and allowed to air to room temperature to obtain calcined carbide slag; The calcined carbide slag is mixed with sodium hydroxide solution and the drained material is used as modified carbide slag.

[0012] Preferably, the method for preparing the ultrafine fly ash is as follows: after mixing fly ash and lauramide, putting them into a ball mill for grinding for 1.5 to 2 hours, and after grinding, passing them through a 400-mesh sieve to obtain ultrafine fly ash, wherein the mass of the lauramide is 2% of the mass of the fly ash.

[0013] Preferably, the composite additive further comprises polyether sulfonated oil and magnesium silicate in a mass ratio of 1:0.5, and the mass of the polyether sulfonated oil is 20% of the mass of the ethylene-vinyl acetate copolymer emulsion.

[0014] Preferably, the blast furnace slag is prepared by crushing and screening blast furnace slag to obtain 0.15-5 mm particles, and drying the particles at 100-105° C. for 1.5-2 h to obtain blast furnace slag.

[0015] In a second aspect, a method for preparing any of the above-mentioned all-solid waste aggregate grouting bodies is provided, which comprises the following steps: S1. Mixing base materials to prepare a cementitious material: adding modified carbide slag, blast furnace slag and ultrafine fly ash into a mixer, stirring at a speed of 140 r / min for 3-5 min, adding water at a water-binder ratio of 0.3-0.35, continuing to stir at a speed of 140 r / min for 3-5 min, then adding pretreated coal gangue, stirring at a stirring speed of 280 r / min for 3-5 min to obtain a cementitious material; S2. Adding a composite modifier to obtain a slurry: adding a composite modifier to the gelling material, stirring at 800 rpm for 10-15 minutes to obtain a slurry; S3. Add pretreated desert sand to the slurry and use a vacuum mixer to stir at -0.08 MPa and 200 r / min for 5 to 10 minutes to obtain a full solid waste aggregate grouting body.

[0016] The beneficial effects of the technical solution provided by this application include: The present application provides an all-solid waste aggregate grouting body and a preparation method thereof, wherein a high-strength skeleton is constructed using solid wastes such as coal gangue, carbide slag, blast furnace slag, and ultrafine fly ash as the base material, wherein the pretreated coal gangue has increased active sites, which together with the carbide slag and blast furnace slag promote the generation of strength phases such as CSH gel and ettringite (AFt); the hydrogenated coconut acid in the composite additive plays a lubricating and drag-reducing role, reducing the friction between the solid waste particles and the desert sand, and cooperates with the dispersing effect of the polyether sulfonated oil to allow the base material and aggregate to be evenly distributed in the slurry; the ethylene-vinyl acetate copolymer emulsion fills the pores in a fluid state in the early stage and improves the cohesiveness of the slurry, so that the grouting body has good construction fluidity to meet the grouting requirements. At the same time, after the pre-treated desert sand is fully combined with the slurry, the slurry can effectively wrap and bond the desert sand particles, and use its own strength and adhesion to achieve better fixation and bonding effects in the desert environment. Through reasonable proportioning and process control, the grouting body can form a synergistic effect with the desert sand, so that the loose desert sand has higher integrity and stability after grouting, making it suitable for reinforcement, repair and other engineering needs in desert sand environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0018] Figure 1 Flow chart of the preparation method of all-solid waste aggregate grouting body provided in this application; Figure 2 The XDR image of the solid waste aggregate grouting specimen prepared in Example 1 provided in this application; Figure 3 The XRD pattern of the solid waste aggregate grouting specimen prepared in Example 1 provided in this application; Figure 4 TG-DSC curve of the solid waste aggregate grouting specimen prepared in Example 1 provided in this application; Figure 5 This is the FTIR change curve of the all-solid waste aggregate grouting specimen prepared in Example 1 provided in this application; Figure 6 These are scanning electron microscope images of the all-solid waste aggregate grouting specimen prepared in Example 1 provided in this application at 3d and 28d. DETAILED DESCRIPTION

[0019] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0020] See also Figures 1 to 6 As shown, the present application provides a full solid waste aggregate grouting body and a preparation method thereof.

[0021] Example 1 The preparation method of the all-solid waste aggregate grouting body provided in this application is: S101, mixing base materials to prepare a cementitious material: adding 200 g of modified carbide slag, 300 g of blast furnace slag, and 200 g of ultrafine fly ash into a blender, stirring at a speed of 140 r / min for 3 min, adding 320 g of water, continuing to stir at a speed of 140 r / min for 3 min, then adding 300 g of pretreated coal gangue, stirring at a stirring speed of 280 r / min for 5 min, to obtain a cementitious material; S102, adding a composite modifier to obtain a slurry: adding 100 g of the composite modifier to the gelling material obtained in S101, stirring at 800 rpm for 10 min to obtain a slurry; S103. Add 400 g of pretreated desert sand to the slurry, and use a vacuum mixer to stir at -0.08 MPa and 200 r / min for 10 minutes to obtain a full solid waste aggregate grouting body.

[0022] In S101, the modified carbide slag is prepared by passing the carbide slag through a 200-mesh sieve, then placing the sieved carbide slag in a muffle furnace for calcining, heating the temperature to 760° C. at a rate of 20° C. / min, and calcining at 760° C. for 2.5 hours. After the calcination is completed, the carbide slag is removed from the muffle furnace and allowed to air cool to room temperature to obtain calcined carbide slag. 300 g of calcined carbide slag was mixed with 100 g of 1 mol / L sodium hydroxide solution, and the drained product was used as modified carbide slag.

[0023] The blast furnace slag preparation method comprises the following steps: taking blast furnace slag, crushing and screening to obtain 0.15-5 mm particles, and drying at 105° C. for 1.5 hours to obtain blast furnace slag.

[0024] The preparation method of ultrafine fly ash is as follows: 300g fly ash and 6g lauramide are mixed, and the mixture is put into a ball mill for grinding for 1.5h. After the grinding, the mixture is sieved through a 400-mesh sieve to obtain ultrafine fly ash.

[0025] The pretreated gangue is prepared by mixing 400 g of gangue with a particle size of 3 to 4.5 cm with 80 g of the modified liquid, stirring the mixture in an 80° C. water bath for 60 min, and then standing and curing the mixture for 24 h to obtain the pretreated gangue. The modified liquid consists of 3g wood vinegar, 2g conchiolin powder and 100g water.

[0026] In S102, the composite modifier is a composition of 30g hydrogenated coconut oil, 30g glucosylrutin, 40g ethylene-vinyl acetate copolymer emulsion, 8g polyether sulfonated oil and 4g magnesium silicate, wherein the solid content of the ethylene-vinyl acetate copolymer emulsion is 50%.

[0027] In S103, the preparation method of pretreated desert sand is as follows: after passing the desert sand through a 30-mesh sieve, soaking it in a 0.1 mol / L oxalic acid solution for 1.5 hours, washing it with clean water until it is neutral, and drying it at 105° C. to obtain the pretreated desert sand.

[0028] Example 2 The difference from Example 1 is that the method for preparing the all-solid waste aggregate grouting body provided in this embodiment is: S201, mixing base materials to prepare a cementitious material: adding 150 g of modified carbide slag, 350 g of blast furnace slag, and 250 g of ultrafine fly ash into a blender, stirring at a speed of 140 r / min for 3 min, adding 320 g of water, continuing to stir at a speed of 140 r / min for 3 min, then adding 250 g of pretreated coal gangue, stirring at a stirring speed of 280 r / min for 5 min, to obtain a cementitious material; S202, adding a composite modifier to obtain a slurry: adding 100 g of the composite modifier to the gelling material obtained in S201, stirring at 800 rpm for 10 min to obtain a slurry; S203. Add 400 g of pretreated desert sand to the slurry, use a vacuum mixer, stir at -0.08 MPa and 200 r / min for 10 min, and obtain a full solid waste aggregate grouting body.

[0029] The preparation method and components of pretreated coal gangue, modified carbide slag, blast furnace slag, ultrafine fly ash, composite modifier, and pretreated desert sand are consistent with those in Example 1.

[0030] Example 3 The difference from Example 1 is that the composite modifier includes 30g hydrogenated coconut oil, 30g glucosylrutin and 40g ethylene-vinyl acetate copolymer emulsion, the composite modifier accounts for 10% of the mass of the base material, and the total actual addition amount is 100g.

[0031] Example 4 The difference from Example 1 is that the composite modifier is 5% of the mass of the base material, and the total addition amount is 50g.

[0032] Example 5 The preparation method of the all-solid waste aggregate grouting body provided in this application is: S501, mixing base materials to prepare a cementitious material: adding 250 g of modified carbide slag, 250 g of blast furnace slag, and 100 g of ultrafine fly ash into a blender, stirring at a speed of 140 r / min for 5 min, adding 300 g of water, continuing to stir at a speed of 140 r / min for 5 min, then adding 400 g of pretreated coal gangue, stirring at a stirring speed of 280 r / min for 3 min, to obtain a cementitious material; S502, adding a composite modifier to obtain a slurry: adding 120 g of a composite modifier to the gelling material obtained in S501, stirring at 800 rpm for 15 min to obtain a slurry; S503. Add 400 g of pretreated desert sand to the slurry, and use a vacuum mixer to stir at -0.08 MPa and 200 r / min for 5 minutes to obtain a full solid waste aggregate grouting body.

[0033] In S501, the modified carbide slag is prepared by passing the carbide slag through a 200-mesh sieve, then placing the sieved carbide slag in a muffle furnace for calcination, heating the temperature to 750° C. at a rate of 20° C. / min, and calcining at 760° C. for 1 hour. After the calcination, the carbide slag is removed from the muffle furnace and allowed to air cool to room temperature to obtain calcined carbide slag. 300 g of calcined carbide slag was mixed with 100 g of 1 mol / L sodium hydroxide solution, and the drained product was used as modified carbide slag.

[0034] The blast furnace slag preparation method comprises the following steps: taking blast furnace slag, crushing and screening to obtain 0.15-5 mm particles, and drying at 100° C. for 2 hours to obtain blast furnace slag.

[0035] The preparation method of ultrafine fly ash is as follows: 300g fly ash and 6g lauramide are mixed, and the mixture is put into a ball mill for grinding for 2h. After the grinding, the mixture is sieved through a 400-mesh sieve to obtain ultrafine fly ash.

[0036] The pretreated gangue was prepared by mixing 450 g of gangue with a particle size of 3 to 4.5 cm with 45 g of the modified liquid, stirring the mixture in an 80°C water bath for 55 minutes, and then allowing the mixture to stand for 24 hours to obtain the pretreated gangue. The modified liquid consists of 3g of wood vinegar, 3g of conchiolin powder and 100g of water.

[0037] In S502, the composite modifier is a composition of 28g hydrogenated coconut oil, 42g glucosylrutin, 56g ethylene-vinyl acetate copolymer emulsion, 11.2g polyether sulfonated oil and 5.6g magnesium silicate, wherein the solid content of the ethylene-vinyl acetate copolymer emulsion is 50%.

[0038] In S503, the preparation method of the pretreated desert sand is as follows: after passing the desert sand through a 30-mesh sieve, soaking it in a 0.1 mol / L oxalic acid solution for 2 hours, washing it with clean water until it is neutral, and drying it at 100° C. to obtain the pretreated desert sand.

[0039] Comparative Example 1 This comparative example differs from Example 1 in that the composite additive is replaced with an equal amount of water.

[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that the pretreated coal gangue is replaced by an equal amount of coal gangue that has not been treated with the modifying liquid, and the composite additive is replaced by an equal amount of water.

[0041] Comparative Example 3 This comparative example differs from Example 1 in that the desert sand is not pretreated, and the pretreated desert sand in S103 is replaced with an equal amount of desert sand.

[0042] The all-solid waste aggregate grouting bodies (hereinafter referred to as grouting bodies) prepared by the preparation methods of Examples 1 to 5 and Comparative Examples 1 to 3 were tested.

[0043] Fluidity test: Referring to GB / T 2419-2005 "Determination of fluidity of cement mortar", pour the grouting body into a truncated cone mold (upper diameter 70mm, lower diameter 100mm, height 60mm), vibrate 25 times and then lift the mold. After 30 seconds, use a caliper to measure the diameters of the bottom surface of the grouting body in two directions perpendicular to each other, and take the average value as the expansion.

[0044] Compressive strength test: Referring to GB / T17671-2021 "Test method for strength of cement mortar (ISO method)", the grouting body is made into a 40mm×40mm×160mm cubic test block. After standard curing (temperature 20±2℃, relative humidity ≥95%) for 28 days, the compressive strength test is carried out using a pressure testing machine at a loading rate of 2.4kN / s. The average value of the 6 test blocks is taken as the 28d compressive strength.

[0045] Shrinkage test: Refer to the drying shrinkage test method specified in GB / T11969-2008, "Test Methods for Properties of Autoclaved Aerated Concrete." Build the grout into a 40mm × 40mm × 160mm cubic specimen. Drill a hole 80mm in diameter and 13mm in depth at each end of the specimen to embed the shrinkage head. After 1 day, immerse the specimen in a constant temperature water bath at (20±2)°C for 72 hours. Measure the length at 28 days. Shrinkage = (initial length - 28-day length) / initial length × 100%.

[0046] The experimental results are shown in Table 1.

[0047] Table 1

[0048] Compared with Example 1, the proportion of pretreated coal gangue and modified carbide slag in Example 2 is reduced, and the strength is reduced. Compared with Example 1, the composite additive in Example 3 lacks polyether sulfonated oil and magnesium silicate, and the fluidity is reduced.

[0049] Comparative Examples 1 and 2 did not add composite additives, and the hydration shrinkage was more obvious and the fluidity decreased. The desert sand in Comparative Example 3 was not pretreated, and the bonding degree between the particles was poor, so the shrinkage rate was larger.

[0050] Furthermore, the compressive strength of the specimens prepared in Example 1 at various ages is shown in Table 2.

[0051] Table 2

[0052] It can be seen from Tables 1 and 2 that Example 1 has better comprehensive performance. The pretreated coal gangue and modified carbide slag can participate in the hydration reaction better. The ethylene-vinyl acetate copolymer emulsion in the composite additive forms an elastic network, which relieves stress while effectively reducing shrinkage. Magnesium silicate stimulates the activity of blast furnace slag and improves the overall strength through the synergistic effect of multiple mechanisms of lubrication, shrinkage prevention and toughening.

[0053] See also Figure 2 As shown, it is an XDR image of the grouting body prepared in Example 1.

[0054] The main mineral component of carbide slag, Ca(OH)2, decomposes at 510°C, then reacts with CO2 in the air, decomposes into CaCO3 at 720°C, and converts into calcium oxide after calcination; coal gangue contains a large amount of silicon oxide and aluminum oxide that can react with calcium oxide, making it more firmly bonded to other base materials, increasing the friction between the all-solid waste large aggregate grouting body and the sandy soil outside the pile body, and further improving the compressive and tensile bearing capacity of the steel pipe pile.

[0055] See also Figures 3 to 5 As shown in the figure, the XRD pattern, TG-DSC curve and FTIR curve of the grouting specimen prepared in Example 1 are shown in the figure. Figure 3 It can be seen that ettringite (AFt) has obvious characteristic peaks at different ages (6h, 1d, 3d, 7d, 28d), and it increases with age, indicating that it is continuously generated over a long period of time, which is beneficial to the consolidation of the strength of the grouting specimen. The filling and cementation of hydration products make the grouting specimen structure dense and improve its load-bearing capacity. Figure 4 It can be seen that as the curing age increases, the mass loss rate gradually decreases; the slower the mass loss rate and the smaller the loss amount in the 200~600℃ stage, the more stable the hydration products are and the denser the structure is. After 600℃, the mass loss rate of the TG curve slows down. The early age (6h~3d) is mainly free water evaporation, indicating that early hydration products (such as AFt) are generated and the fluidity is guaranteed. In the middle period (3d~7d), the hydration products tend to be stable. In the later period (7d~28d), the grouting specimens have formed a stable and dense structure. Figure 5 You can know that 800~1200cm -1 The characteristic absorption of silicate hydration products such as CSH gel gradually becomes sharper and the intensity increases with age, indicating that CSH gel is continuously generated and the crystallinity increases. The silicate hydration reaction of the grouting body continues and the structure gradually becomes denser.

[0056] as well as, Figure 6 These are the scanning electron microscope (SEM) images of the grouting specimens prepared in Example 1 at 3d and 28d.

[0057] The foregoing is merely a list of specific embodiments of the present application, intended to enable those skilled in the art to understand or implement the present application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application is not limited to the embodiments shown herein, but is intended to conform to the broadest scope consistent with the principles and novel features of the present application.

Claims

1. A solid waste aggregate grouting body, characterized in that: It consists of a slurry and pre-treated desert sand: The slurry includes a base material, a composite additive and water; According to the weight ratio, the base material includes 25-40 parts of pretreated coal gangue, 15-25 parts of modified carbide slag, 25-35 parts of blast furnace slag, and 10-25 parts of ultrafine fly ash; The mass of the composite additive is 5-12% of the mass of the base material, and the composite additive includes hydrogenated coconut oil, glucosylrutin and ethylene-vinyl acetate copolymer emulsion in a mass ratio of (2-3):3:4; The ratio of the mass of the water to the mass of the base material is (0.3-0.35):1; The mass of the pretreated desert sand is 40% of the slurry.

2. The all-solid waste aggregate grouting body according to claim 1, characterized in that: The method for preparing pretreated desert sand comprises the following steps: After passing the desert sand through a 30-mesh sieve, the sand was soaked in a 0.1 mol / L oxalic acid solution for 1.5 to 2 h, rinsed with clean water until neutral, and dried at 100 to 105°C to obtain pretreated desert sand.

3. The all-solid waste aggregate grouting body according to claim 1, characterized in that: The preparation of the pretreated coal gangue comprises the following steps: The gangue and the modifying liquid were mixed in a mass ratio of 1:(0.1-0.25), stirred in an 80°C water bath for 55-60 minutes, and then allowed to stand for 24 hours to obtain pretreated gangue; The modified liquid comprises wood vinegar, conchiolin powder and water in a mass ratio of 3:(2-3):

100.

4. The all-solid waste aggregate grouting body according to claim 3, characterized in that: The particle size of the coal gangue is 3-4.5 cm.

5. The all-solid waste aggregate grouting body according to claim 1, characterized in that: The modified carbide slag is prepared by passing the carbide slag through a 200-mesh sieve, then placing the sieved carbide slag in a muffle furnace for calcination, heating the temperature to 750-760° C. at a rate of 20° C. / min, and calcining the carbide slag at 750-760° C. for 1-2.5 hours. After the calcination is completed, the carbide slag is taken out of the muffle furnace and aired to room temperature to obtain calcined carbide slag. The calcined carbide slag is mixed with sodium hydroxide solution and the drained material is used as modified carbide slag.

6. The all-solid waste aggregate grouting body according to claim 1, characterized in that: The method for preparing the ultrafine fly ash comprises the following steps: mixing fly ash and lauramide, putting the mixture into a ball mill and grinding the mixture for 1.5 to 2 hours; and passing the mixture through a 400-mesh sieve after grinding to obtain the ultrafine fly ash, wherein the mass of the lauramide is 2% of the mass of the fly ash.

7. The all-solid waste aggregate grouting body according to claim 1, characterized in that: The composite additive further comprises polyether sulfonated oil and magnesium silicate in a mass ratio of 1:0.5, wherein the mass of the polyether sulfonated oil is 20% of the mass of the ethylene-vinyl acetate copolymer emulsion.

8. The all-solid waste aggregate grouting body according to claim 1, characterized in that: The preparation method of the blast furnace slag comprises the following steps: taking blast furnace slag, crushing and screening to obtain 0.15-5 mm particles, and drying at 100-105° C. for 1.5-2 hours to obtain blast furnace slag.

9. A method for preparing the all-solid waste aggregate grouting body according to any one of claims 1 to 8, characterized in that: It includes the following steps: S1. Mixing base materials to prepare a cementitious material: adding modified carbide slag, blast furnace slag and ultrafine fly ash into a mixer, stirring at a speed of 140 r / min for 3-5 min, adding water at a water-binder ratio of 0.3-0.35, continuing to stir at a speed of 140 r / min for 3-5 min, then adding pretreated coal gangue, stirring at a stirring speed of 280 r / min for 3-5 min to obtain a cementitious material; S2. Adding a composite modifier to obtain a slurry: adding a composite modifier to the gelling material, stirring at 800 rpm for 10-15 minutes to obtain a slurry; S3. Add pretreated desert sand to the slurry and use a vacuum mixer to stir at -0.08 MPa and 200 r / min for 5 to 10 minutes to obtain a full solid waste aggregate grouting body.

Citation Information

Patent Citations

  • Modification method of brick-making material

    CN102442793A

  • High-strength polishing chip

    CN106630972A

  • Micro-expansion grouting material and preparation method thereof

    CN108203281A

  • Anti-crack dry-mixed mortar taking Yellow River sand as raw material and preparation process of anti-crack dry-mixed mortar

    CN117417159A

  • All-solid-waste-based cementing material for stabilizing aeolian sand as well as preparation method and application of all-solid-waste-based cementing material

    CN118754531A