A closed-pore lithium battery separator with high ionic conductivity and its preparation method
By filling the pore structure of the PE-based membrane with modified polyethylene oxide derivatives, the problem of slow pore-closing response of the PE membrane was solved, achieving high ionic conductivity and rapid pore-closing, thus improving the safety performance of lithium batteries.
Patent Information
- Application Number
- CN202510859377.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-06-25
AI Technical Summary
Existing PE separators have a slow pore-closing response in lithium batteries, which cannot prevent heat accumulation in time and affects ionic conductivity, thus failing to meet the requirements of high-performance lithium batteries.
A modified polyethylene oxide derivative is filled into the pore structure of a PE-based membrane. The modified polyethylene oxide derivative contains N-isopropylacrylamide segments, fluorinated groups, and thiourea groups. Through a specific chemical reaction, PEO-NIPAM-BMIM is formed, which enhances its thermal responsiveness and ion conduction performance at high temperatures.
This technology enables rapid pore closure of the PE membrane at high temperatures, maintains high ionic conductivity, and improves the structural stability and mechanical strength of the membrane, preventing rupture.
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery separator technology, specifically to a closed-pore lithium battery separator with high ionic conductivity and its preparation method. Background Technology
[0002] In lithium-ion batteries, the separator plays a crucial role in isolating the positive and negative electrodes, preventing short circuits, and allowing lithium ions to pass through. Polyethylene (PE) separators are currently one of the most widely used lithium-ion battery separators. However, existing PE separators have significant shortcomings in addressing battery thermal runaway issues. Their pore-closing response is slow, failing to promptly prevent further heat accumulation inside the battery. Moreover, the pore-closing process often leads to impaired ionic conductivity, affecting battery performance.
[0003] While some studies have attempted to improve the performance of PE separators by introducing water-soluble, ion-conducting polymers during the aqueous coating process, these methods still have limitations in terms of increasing pore-closing speed and maintaining high ionic conductivity, and cannot meet the stringent requirements of high-performance lithium batteries for separators. Summary of the Invention
[0004] The purpose of this invention is to provide a closed-pore lithium battery separator with high ionic conductivity and its preparation method, thereby solving the following technical problems:
[0005] How to achieve rapid thermal pore closure of PE membranes while maintaining high ionic conductivity.
[0006] The objective of this invention can be achieved through the following technical solutions:
[0007] In a first aspect, the present invention discloses a closed-pore lithium battery separator with high ionic conductivity, comprising a PE base membrane, wherein the pore structure of the PE base membrane is filled with a modified polyethylene oxide derivative, wherein the modified polyethylene oxide derivative contains an N-isopropylacrylamide segment, a fluorinated group and a thiourea group.
[0008] Furthermore, the preparation method of the modified polyethylene oxide derivative includes the following steps:
[0009] Step 1: Dissolve polyethylene oxide (PEO) and N-isopropylacrylamide (NIPAM) in an organic solvent at a molar ratio of (10-50):1, add an initiator, and react at 60-80℃ for 2-6 hours under nitrogen protection to obtain reaction solution A; during the reaction, N-isopropylacrylamide is grafted onto polyethylene oxide through polymerization to form PEO-NIPAM.
[0010] Step 2: Add 1-butyl-3-methylimidazolium hexafluorophosphate (BMIM) to reaction solution A, add a catalyst, and react at 70-90℃ for 3-8 hours to obtain reaction solution B; during the reaction, the functionalized groups in 1-butyl-3-methylimidazolium hexafluorophosphate are grafted onto the molecular chain of PEO-N IPAM to form PEO-NIPAM-BMIM.
[0011] Step 3: Add isothiocyanate and catalyst to reaction solution B, react at 70-80℃ for 2 hours, precipitate, filter, wash and dry to obtain modified polyethylene oxide derivative.
[0012] Preferably, in step 1, the molar ratio of polyethylene oxide to N-isopropylacrylamide is 30:1.
[0013] Preferably, in step 1, the reaction temperature is 70°C and the reaction time is 4 hours.
[0014] Preferably, in step 2, the reaction temperature is 80°C and the reaction time is 5 hours.
[0015] Preferably, in step 3, the reaction temperature is 75°C and the reaction time is 1.5 h.
[0016] Further, in step 1, the initiator is any one or any mixture of any combination of azobisisobutyronitrile, azobisisoheptanenitrile, and dimethyl azobisisobutyrate in any proportion.
[0017] Preferably, in step 1, the initiator is azobisisobutyronitrile.
[0018] Further, in step 1, the mass ratio of the polyethylene oxide to N-isopropylacrylamide and the volume ratio of the organic solvent is 1 g:(10-15) mL.
[0019] Preferably, the organic solvent is dimethyl sulfoxide.
[0020] Preferably, in step 1, the mass ratio of the polyethylene oxide to N-isopropylacrylamide and the volume ratio of the organic solvent is 1 g: 12 mL.
[0021] Further, in step 2, the molar ratio of the reaction product in reaction solution A to 1-butyl-3-methylimidazolium hexafluorophosphate is 1:(0.1-0.5).
[0022] Preferably, in step 2, the molar ratio of the reaction product in reaction solution A to 1-butyl-3-methylimidazolium hexafluorophosphate is 1:0.3.
[0023] Further, in step 2, the catalyst is any one or a mixture of any combination of benzoyl peroxide, di-tert-butyl peroxide, and tert-butyl peroxide in any proportion.
[0024] Preferably, in step 2, the catalyst is benzoyl peroxide.
[0025] Further, in step 3, the molar ratio of the reaction product to isothiocyanate in the reaction solution B is 1:(0.2-0.6).
[0026] Preferably, in step 3, the molar ratio of the reaction product to isothiocyanate in the reaction solution B is 1:0.4.
[0027] Further, in step 3, the catalyst is any one or a mixture of any combination of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, and di(dodecyl sulfide)dibutyltin.
[0028] Preferably, in step 3, the catalyst is dibutyltin dilaurate.
[0029] Based on this, a preferred method for preparing modified polyethylene oxide derivatives is obtained, comprising the following steps:
[0030] Step 1: Dissolve 3 mol of polyethylene oxide and 0.1 mol of N-isopropylacrylamide in dimethyl sulfoxide, add azobisisobutyronitrile, and react at 70°C for 4 h under nitrogen protection to obtain reaction solution A containing PEO-NIPAM.
[0031] Step 2: Add 0.9 mol of 1-butyl-3-methylimidazolium hexafluorophosphate directly to reaction solution A, add benzoyl peroxide, and react at 80℃ for 5 h to obtain reaction solution B containing PEO-NIPAM-BM IM;
[0032] Step 3: Add 1.2 mol of isothiocyanate directly to reaction solution B, add dibutyltin dilaurate, react at 70-80℃ for 2 h, precipitate, filter, wash, and dry to obtain modified polyethylene oxide derivative.
[0033] Secondly, the present invention also discloses a method for preparing a closed-pore lithium battery separator with high ionic conductivity as described above, comprising the following steps:
[0034] S1. Dissolve the modified polyethylene oxide derivative in water to form a coating solution with a mass fraction of 10-12%;
[0035] S2. The coating liquid is uniformly coated on the PE base film with a coating thickness of 1-2 μm. After vacuum drying, a closed-cell lithium battery separator with high ionic conductivity is obtained.
[0036] Preferably, in step S1, the mass fraction of the coating liquid is 10-12%.
[0037] Furthermore, in step S2, the thickness of the PE base film is 12-20 μm.
[0038] Furthermore, in step S2, the vacuum drying temperature is 75-90℃ and the time is 1.5-2.5h.
[0039] Preferably, in step S2, the vacuum drying temperature is 85°C and the time is 2 hours.
[0040] The beneficial effects of this invention are:
[0041] (1) The high ionic conductivity closed-pore lithium battery separator of the present invention is filled with modified polyethylene oxide derivatives, which introduce N-isopropylacrylamide segments, fluorinated groups and thiourea groups. The N-isopropylacrylamide segments have a low critical dissolution temperature. When the temperature rises to near the critical dissolution temperature, its molecular chain undergoes a conformational transformation from extension to coiling. In lithium battery separator applications, this temperature responsiveness can be combined with the thermal runaway process of the battery. At normal operating temperature, the N-isopropylacrylamide segments extend, providing a good transport channel for lithium ions and ensuring high ionic conductivity. When the battery temperature rises to 130°C, the N-isopropylacrylamide segments rapidly coil and interact with the polyethylene oxide backbone, promoting the rapid closure of the separator pores.
[0042] (2) The fluorinated groups in the modified polyethylene oxide derivatives were obtained by introducing 1-butyl-3-methylimidazolium hexafluorophosphate. 1-Butyl-3-methylimidazolium hexafluorophosphate is an ionic liquid with excellent ionic conductivity and thermal stability, which can significantly improve the ionic conductivity of the membrane. Simultaneously, the interaction between the functionalized groups and the polyethylene oxide backbone enhances the structural stability of the membrane, helping to maintain its integrity at high temperatures and preventing it from rupturing due to thermal expansion. This improves its conductivity and strength properties.
[0043] (3) The thiourea groups in the modified polyethylene oxide derivatives form moderate hydrogen bonds with water molecules or themselves at room temperature. At a high temperature of 130°C, the water evaporates or migrates. At this time, a stronger and denser hydrogen bond network will be formed between the thiourea groups, resulting in physical cross-linking of the PEO chains, a sharp increase in viscosity, and further promotion of pore closure. Detailed Implementation
[0044] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0045] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0046] Preparation Example 1
[0047] The modified polyethylene oxide derivative was prepared by following these steps:
[0048] Step 1: In a stirrer, 132 g (3 mol) of polyethylene oxide and 11.316 g (0.1 mol) of N-isopropylacrylamide were dissolved in 1720 mL of dimethyl sulfoxide, and azobisisobutyronitrile was added. The mixture was reacted at 70 °C for 4 h under nitrogen protection to obtain reaction solution A.
[0049] Step 2: Add 266.6 g (0.9 mol) of 1-butyl-3-methylimidazolium hexafluorophosphate and 2.12 g of benzoyl peroxide directly to reaction solution A, and react at 80 °C for 5 h to obtain reaction solution B;
[0050] Step 3: Add 60.11 g (1.2 mol) of isothiocyanate and 0.95 g of dibutyltin dilaurate directly to reaction solution B, and react at 75 °C for 2 h to obtain reaction solution C;
[0051] Step 4: After precipitating reaction solution C for 2 hours, filter it through a funnel. Wash the filter material repeatedly with diethyl ether and place it in a vacuum drying oven to dry at 60°C for 5 hours to obtain the modified polyethylene oxide derivative.
[0052] Preparation Example 2
[0053] The modified polyethylene oxide derivative was prepared by following these steps:
[0054] Step 1: In a stirrer, 44 g (1 mol) of polyethylene oxide and 11.316 g (0.1 mol) of N-isopropylacrylamide were dissolved in 664 mL of dimethyl sulfoxide, and azobisisobutyronitrile was added. The mixture was reacted at 70 °C for 3 h under nitrogen protection to obtain reaction solution A.
[0055] Step 2: Add 29.62 g (0.1 mol) of 1-butyl-3-methylimidazolium hexafluorophosphate and 1.42 g of benzoyl peroxide directly to reaction solution A, and react at 80 °C for 3.5 h to obtain reaction solution B;
[0056] Step 3: Add 11.82 g (0.2 mol) of isothiocyanate and 0.59 g of dibutyltin dilaurate directly to reaction solution B, and react at 70 °C for 2 h to obtain reaction solution C;
[0057] Step 4: After precipitating reaction solution C for 2 hours, filter it through a funnel. Wash the filter material repeatedly with diethyl ether and place it in a vacuum drying oven to dry at 60°C for 5 hours to obtain the modified polyethylene oxide derivative.
[0058] Preparation Example 3
[0059] The modified polyethylene oxide derivative was prepared by following these steps:
[0060] Step 1: In a stirrer, 220 g (5 mol) of polyethylene oxide and 11.316 g (0.1 mol) of N-isopropylacrylamide were dissolved in 2776 mL of dimethyl sulfoxide, and azobisisobutyronitrile was added. The mixture was reacted at 70 °C for 6 h under nitrogen protection to obtain reaction solution A.
[0061] Step 2: Add 740g (2.5mol) of 1-butyl-3-methylimidazolium hexafluorophosphate and 3.41g of benzoyl peroxide directly to reaction solution A, and react at 80℃ for 5h to obtain reaction solution B;
[0062] Step 3: Add 177.3 g (3 mol) of isothiocyanate and 2.49 g of dibutyltin dilaurate directly to reaction solution B, and react at 75 °C for 2 h to obtain reaction solution C;
[0063] Step 4: After precipitating reaction solution C for 2 hours, filter it through a funnel. Wash the filter material repeatedly with diethyl ether and place it in a vacuum drying oven to dry at 60°C for 5 hours to obtain the modified polyethylene oxide derivative.
[0064] Comparative Preparation Example 1
[0065] The modified polyethylene oxide derivative was prepared by omitting step 2, while keeping the other steps and conditions the same, in order to obtain the modified polyethylene oxide derivative.
[0066] Comparative Preparation Example 2
[0067] The modified polyethylene oxide derivative was prepared by omitting step 3, while keeping the other steps and conditions the same, in order to obtain the modified polyethylene oxide derivative.
[0068] Example 1
[0069] The preparation of a closed-pore lithium battery separator with high ionic conductivity is carried out according to the following steps:
[0070] S1. Dissolve 11g of the modified polyethylene oxide derivative prepared in Example 1 in 89g of water to form a coating solution;
[0071] S2. The coating liquid is uniformly coated onto a PE base film with a length of 6cm, a width of 4cm, and a thickness of 15um using a separator coating machine. The coating thickness is 1.5um. Then, it is placed in a vacuum dryer and dried at 85℃ for 2 hours to obtain a closed-cell lithium battery separator with high ionic conductivity.
[0072] Example 2
[0073] The preparation of a closed-pore lithium battery separator with high ionic conductivity is carried out according to the following steps:
[0074] S1. Dissolve 10g of the modified polyethylene oxide derivative prepared in Example 1 in 90g of water to form a coating solution;
[0075] S2. The coating liquid is uniformly coated onto a PE base film with a length of 6cm, a width of 4cm, and a thickness of 15um using a separator coating machine. The coating thickness is 1.5um. Then, it is placed in a vacuum dryer and dried at 85℃ for 2 hours to obtain a closed-cell lithium battery separator with high ionic conductivity.
[0076] Example 3
[0077] The preparation of a closed-pore lithium battery separator with high ionic conductivity is carried out according to the following steps:
[0078] S1. Dissolve 12g of the modified polyethylene oxide derivative prepared in Example 1 in 88g of water to form a coating solution;
[0079] S2. The coating liquid is uniformly coated onto a PE base film with a length of 6cm, a width of 4cm, and a thickness of 15um using a separator coating machine. The coating thickness is 1.5um. Then, it is placed in a vacuum dryer and dried at 85℃ for 2 hours to obtain a closed-cell lithium battery separator with high ionic conductivity.
[0080] Example 4
[0081] The preparation of a closed-pore lithium battery separator with high ionic conductivity is carried out according to the following steps:
[0082] S1. Dissolve 11g of the modified polyethylene oxide derivative prepared in Example 2 in 89g of water to form a coating solution;
[0083] S2. The coating liquid is uniformly coated onto the PE base film using a separator coating machine to a coating thickness of 1.5 μm. Then, it is placed in a vacuum dryer and dried at 85°C for 2 hours to obtain a closed-cell lithium battery separator with high ionic conductivity.
[0084] Example 5
[0085] The preparation of a closed-pore lithium battery separator with high ionic conductivity is carried out according to the following steps:
[0086] S1. Dissolve 11g of the modified polyethylene oxide derivative prepared in Example 3 in 89g of water to form a coating solution;
[0087] S2. The coating liquid is uniformly coated onto the PE base film using a separator coating machine to a coating thickness of 1.5 μm. Then, it is placed in a vacuum dryer and dried at 85°C for 2 hours to obtain a closed-cell lithium battery separator with high ionic conductivity.
[0088] Comparative Example 1
[0089] The preparation of a closed-cell lithium battery separator differs from Example 1 only in that the modified polyethylene oxide derivative obtained in Preparation Example 1 is replaced with the modified polyethylene oxide derivative obtained in Comparative Preparation Example 1. All other steps and conditions remain the same, ultimately yielding a closed-cell lithium battery separator with high ionic conductivity.
[0090] Comparative Example 2
[0091] The preparation of a closed-cell lithium battery separator differs from Example 1 only in that the modified polyethylene oxide derivative obtained in Example 1 is replaced with the modified polyethylene oxide derivative obtained in Comparative Example 2, while the other steps and conditions remain the same, ultimately yielding a closed-cell lithium battery separator with high ionic conductivity.
[0092] Comparative Example 3
[0093] The preparation of a closed-cell lithium battery separator differs from Example 1 only in that the modified polyethylene oxide derivative obtained in Example 1 is replaced with polyethylene oxide, while the other steps and conditions remain the same, ultimately yielding a closed-cell lithium battery separator with high ionic conductivity.
[0094] The performance of the closed-cell lithium battery separators prepared in Examples 1-5 and Comparative Examples 1-3 was tested using the following methods:
[0095] Closed-pore response time test: The diaphragm was tested using a thermomechanical analyzer (TMA) and the time it took for the pores of the diaphragm to begin closing during the heating process was recorded.
[0096] Ionic conductivity test: The membrane was assembled into a symmetrical cell, and the ionic conductivity of the membrane at different temperatures was tested by electrochemical impedance spectroscopy (EIS).
[0097] Mechanical strength test: The diaphragm is subjected to tensile test using a tensile testing machine to measure the tensile strength and elongation at break of the diaphragm.
[0098] The test results are listed in Table 1, as follows:
[0099] Table 1
[0100] Closed-cell response time / s (130℃) <![CDATA[Ionic conductivity / 10 -3 S / cm (25°C)]]> Tensile strength / MPa Example 1 55 1.8 25.6 Example 2 58 1.9 24.5 Example 3 58 1.9 24.6 Example 4 57 2.0 24.8 Example 5 59 2.0 24.5 Comparative Example 1 78 2.9 27.9 Comparative Example 2 85 2.8 28.5 Comparative Example 3 99 3.1 29.7
[0101] Analysis of the data in Table 1 shows that, compared with Comparative Examples 1-3, the closed-cell lithium battery separators with high ionic conductivity in Examples 1-5 have significantly faster response times at 130°C, and their conductivity and strength performance are significantly better.
[0102] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the claims of this invention should still fall within the patent coverage of this invention.
Claims
1. A high ionic conductivity closed pore lithium battery separator comprising a PE base film, characterized in that, The PE-based membrane has a porous structure filled with a modified polyethylene oxide derivative, which contains N-isopropylacrylamide segments, fluorinated groups, and thiourea groups. The preparation method of the modified polyethylene oxide derivative includes the following steps: Step 1: Dissolve polyethylene oxide and N-isopropylacrylamide in an organic solvent at a molar ratio of (10-50):1, add an initiator, and react at 60-80℃ for 2-6 hours under nitrogen protection to obtain reaction solution A; Step 2: Add 1-butyl-3-methylimidazolium hexafluorophosphate and a catalyst to reaction solution A, and react at 70-90℃ for 3-8 hours to obtain reaction solution B; Step 3: Add isothiocyanate and catalyst to reaction solution B, react at 70-80℃ for 2 hours, precipitate, filter, wash and dry to obtain modified polyethylene oxide derivative.
2. The high ionic conductivity, closed-pore lithium battery separator of claim 1, wherein, In step 1, the initiator is any one or any mixture of any combination of azobisisobutyronitrile, azobisisoheptanenitrile, and dimethyl azobisisobutyrate in any proportion.
3. The high ionic conductivity, closed-pore lithium battery separator of claim 1, wherein, In step 1, the mass ratio of the polyethylene oxide to N-isopropylacrylamide and the volume ratio of the organic solvent is 1 g:(10-15) mL.
4. The closed-cell lithium battery separator with high ionic conductivity according to claim 1, characterized in that, In step 2, the molar ratio of the reaction product in reaction solution A to 1-butyl-3-methylimidazolium hexafluorophosphate is 1:(0.1-0.5).
5. The closed-cell lithium battery separator with high ionic conductivity according to claim 1, characterized in that, In step 2, the catalyst is any one or any mixture of any combination of benzoyl peroxide, di-tert-butyl peroxide, and tert-butyl peroxide in any proportion.
6. The closed-cell lithium battery separator with high ionic conductivity according to claim 1, characterized in that, In step 3, the molar ratio of the reaction product to isothiocyanate in the reaction solution B is 1:(0.2-0.6).
7. The closed-cell lithium battery separator with high ionic conductivity according to claim 1, characterized in that, In step 3, the catalyst is any one or a mixture of any combination of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, and di(dodecyl sulfide)dibutyltin.
8. A method for preparing a closed-cell lithium battery separator with high ionic conductivity according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Dissolve the modified polyethylene oxide derivative in water to form a coating solution with a mass fraction of 10-12%; S2. The coating solution is uniformly coated on the PE base film with a coating thickness of 1-2 μm. After vacuum drying, a closed-cell lithium battery separator with high ionic conductivity is obtained.
9. The method for preparing a closed-pore lithium battery separator with high ionic conductivity according to claim 8, characterized in that, In step S2, the vacuum drying temperature is 75-90℃ and the time is 1.5-2.5h.
Citation Information
Patent Citations
Diaphragm, method for preparing diaphragm and secondary battery comprising diaphragm
CN105789538A
Protein-adsorption-resistant self-cleaning block copolymer as well as preparation method and application thereof
CN111533865A