Graphene micro-nano cavity TIM film and preparation method thereof

By creating grooves on the graphene oxide film and inducing their vertical arrangement, a graphene micro-nanocavity structure is formed, which solves the problem of low longitudinal thermal conductivity of graphene materials and achieves efficient heat dissipation performance improvement.

CN120749023APending Publication Date: 2025-10-03GUANGDONG MORION NANOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510955297.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-11
Publication Date
2025-10-03

AI Technical Summary

Technical Problem

The existing graphene material has a low longitudinal thermal conductivity among TIM materials, which makes it difficult to meet the heat dissipation requirements of high-power usage scenarios.

Method used

By applying downward pressure in the thickness direction of the graphene oxide film to create non-penetrating grooves, the graphene oxide is induced to align in a direction perpendicular to the plane, and a graphene micro-nanocavity structure is formed through self-assembly reaction, thereby enhancing the longitudinal thermal conductivity.

Benefits of technology

The longitudinal thermal conductivity of the graphene micro-nano cavity TIM film is improved, the heat dissipation efficiency is enhanced, and it is suitable for thermal management of high-power chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120749023A_ABST
    Figure CN120749023A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing method of a graphene micro-nano cavity TIM film, which at least comprises the following steps: 1) first coating: coating a substrate with graphene oxide slurry to obtain a primary coating film; (2) applying downward pressure in the thickness direction of the primary coating film to manufacture a non-penetrating groove, carrying out primary drying treatment, and drying the primary coating film until the thickness of the primary coating film is 40-75% of that of the primary coating film before drying; (3) secondary coating is conducted, specifically, the surface, provided with the grooves, of the primary coating film is coated with the graphene oxide slurry again, a secondary coating film is obtained, and the thickness of the primary coating film is larger than that of the secondary coating film; according to the graphene micro-nano cavity TIM film and the preparation method of the graphene micro-nano cavity TIM film, the non-penetrating grooves are manufactured so that graphene oxide can be directionally arranged in the groove mode, and the longitudinal heat conduction performance of the TIM film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of thermal management, and in particular to a graphene micro-nano cavity TIM film and a preparation method thereof. Background Art

[0002] With the development of science and technology, artificial intelligence (AI), driven by the synergy of algorithms, computing power, and data, has achieved technological breakthroughs and has found mature applications in healthcare, intelligent manufacturing, transportation, and urban management. As chip computing power increases, high-power operation generates significant heat. When this heat cannot be removed promptly, it accumulates, directly impacting chip performance, reliability, and even the security of the entire system. For these reasons, chip cooling is crucial. A good cooling system can dissipate heat more quickly, ensuring the chip operates at a safe temperature, thereby enabling higher sustained computing power.

[0003] Currently, chip heat dissipation is primarily achieved through metal heat sinks. TIM material is used to fill the gaps between the chip and the metal heat sink to reduce interfacial thermal resistance and improve heat dissipation efficiency. Traditional TIM materials primarily include thermal grease and thermal pads. Graphene, as an emerging material, is well-suited for use as a TIM material due to its excellent in-plane thermal conductivity and compression resilience. However, the generally low longitudinal thermal conductivity has hindered the application of graphene in TIM materials, making it difficult to meet the heat dissipation requirements of high-power scenarios. Summary of the Invention

[0004] In order to solve one or more technical problems, the first object of this application is to provide a method for preparing a graphene micro-nanocavity TIM film. By applying downward pressure along the thickness direction to induce the graphene oxide film to align perpendicular to the plane, and simultaneously creating non-penetrating grooves to allow the graphene oxide to align along the grooves, the longitudinal thermal conductivity of the TIM film is improved. Specifically: The method comprises at least the following steps: 1) coating a graphene oxide slurry on a substrate to obtain a primary coating film by first coating; 2) applying downward pressure along the thickness direction of the primary coating film to form a non-penetrating groove, performing a first drying treatment, and drying the primary coating film to a thickness of 40%-75% of that before drying; 3) coating a second time, coating the surface of the primary coating film with the groove with the graphene oxide slurry again to obtain a secondary coating film; 4) performing a second drying treatment on the secondary coating film to obtain a graphene oxide film; and 5) sequentially subjecting the graphene oxide film to foaming and heat treatment to obtain a graphene micro-nanocavity TIM film.

[0005] Applying downward pressure along the thickness direction of the primary coating film induces the graphene at the stressed location to change direction, causing the graphene oxide to align perpendicular to the plane during the self-assembly reaction, which is beneficial for improving the vertical thermal conductivity. At the same time, creating non-penetrating grooves on the surface of the primary coating film can provide a channel for the graphene oxide slurry applied for the second time to align along the thickness direction. After the second coating, the graphene oxide slurry still maintains fluidity and flows into the grooves along the thickness direction. At the same time, utilizing the characteristics of graphene oxide self-assembly and graphene wall-attached growth, the portion of the graphene oxide slurry that flows into the groove after the second coating self-assembles along the thickness direction, changing its self-assembly direction and enhancing the thermal conductivity in the longitudinal direction.

[0006] In a further technical solution, the grooves are formed by cutting the primary coating film along its thickness, thereby forming a plurality of grooves spaced apart on the surface of the primary coating film. The cutting tool may be a wire, plate, or cutter, or may be a pre-set mold or machine tool. Any tool suitable for cutting grooves may be used.

[0007] In a further technical solution, the first drying process is performed at a temperature of 25°C to 65°C and for a drying time of 1 to 12 hours, drying the primary coating film to a thickness of 40% to 75% of its pre-drying thickness. The purpose of controlling the first drying process conditions is to keep the primary coating film in a dry, semi-formed state.

[0008] In a further technical solution, the width of the groove is set to 0.02 mm to 1 mm. The spacing between parallel and adjacent grooves is set to 0.02 mm to 1 mm, and the spacing between adjacent grooves may be the same or different. The cutting depth of the groove is less than the thickness of the primary coating film, and the cutting depth of the groove is 10-200 μm less than the thickness of the primary coating film.

[0009] In a further technical solution, the extension direction of the groove is perpendicular to the coating direction of the primary coating film; or the extension direction of the groove is parallel to the coating direction of the primary coating film; or part of the groove is perpendicular to the coating direction of the primary coating film, and the extension direction of part of the groove is parallel to the coating direction of the primary coating film.

[0010] The function of the grooves is to provide a heat conduction path along the thickness direction. Therefore, the grooves must be open in the thickness direction. The grooves can extend in the same direction as the coating direction, perpendicular to the coating direction, or in any direction. However, to ensure the accuracy of the groove dimensions and operability, the grooves are preferably perpendicular to the coating direction, parallel to the coating direction, or both.

[0011] In a further technical solution, the graphene oxide slurry has a solids content of 3%-7% and a carbon-oxygen ratio of 1.2-3:1. Solids content refers to the mass percentage of graphene oxide in the graphene oxide slurry. If the solids content is too high, the slurry viscosity increases, making it too viscous and difficult to coat evenly. On the other hand, if the solids content is too low, the slurry has strong flowability, making it difficult to coat and form a film, and subsequent drying is difficult.

[0012] In a further technical solution, the graphene oxide slurry is applied at a coating speed of 5-60 mm / s during the first coating process, preferably 10-40 mm / s. The core of the coating process is controlling coating thickness and uniformity, and speed directly impacts both. While ensuring a smooth graphene oxide film surface and increasing production capacity, a coating speed of 5-60 mm / s is a reasonable range.

[0013] In a further technical solution, the thickness of the first coating is greater than that of the second coating. The key to improving longitudinal thermal conductivity lies in inducing the graphene oxide to align along the thickness of the coating film. A thicker first coating provides more space for graphene oxide to self-assemble along the thickness direction (i.e., longitudinal direction), which further helps improve longitudinal thermal conductivity. Furthermore, the second coating is primarily used to fill defects, maintaining a smooth secondary coating film. During the second coating process, the graphene oxide slurry can be cast into the grooves. The principle of graphene oxide adhering to the wall growth further helps improve longitudinal thermal conductivity.

[0014] In a further technical solution, during the second drying step, the drying temperature is set to 45°C-65°C, the ambient humidity is controlled at 45%-65% RH, and the drying time is set to 3-10 hours. By controlling the ambient temperature and humidity, the secondary coating film is completely dried. During the second drying process, the evaporation of water promotes the self-assembly reaction of the graphene oxide, forming a graphene oxide film with a vertically oriented structure.

[0015] Another object of the present application is to provide a graphene micro-nano cavity TIM film obtained by the above preparation method; the density of the graphene micro-nano cavity TIM film is ≥0.1g / cm 3, longitudinal thermal conductivity ≥ 15W / (mK), preferably, longitudinal thermal conductivity ≥ 20W / (mK); when the thickness of the graphene micro-nano cavity thermal conductive film is 1mm±0.3mm, the transient compressive stress at 80% compression is ≤ 130psi, and the static compressive stress at 80% compression is ≤ 50Psi. The graphene micro-nano cavity TIM film provided in this application partially chemically reduces the graphene oxide film through a foaming process. The gas released during the chemical reduction process generates micron- and nano-scale cavities inside the film material, thereby obtaining excellent compression rebound performance and being able to fill microscopic unevenness and gaps. It easily deforms and flows under the applied installation pressure to maximize the actual contact area and can effectively fill microscopic pores. Thermal resistance is a comprehensive indicator that measures the ability of the entire interface to hinder heat transfer. The graphene micro-nanocavity TIM film provided in this application not only has the high in-plane thermal conductivity of graphene itself, but also has higher thermal conductivity in the longitudinal direction compared to traditional TIM materials. At the same time, the thickness is controllable, and it has good compression performance and low interface thermal resistance at the thinnest thickness possible, making it an ideal thermal interface material. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0017] Figure 1 This is the method for preparing the groove in step 2) of the preparation method disclosed in the present invention.

[0018] Figure 2 This is a real picture of the front side (groove side) of the graphene TIM film prepared in Example 1 of the present invention.

[0019] Figure 3 This is a real picture of the reverse side of the graphene TIM film prepared in Example 1 of the invention.

[0020] Figure 4 This is a real picture of the front side (groove side) of the graphene TIM film prepared in Example 2 of the present invention.

[0021] Figure 5 This is a real picture of the reverse side of the graphene TIM film prepared in Inventive Example 2.

[0022] Figure 6 This is a compression characteristic test curve diagram of Example 2 of the present invention. DETAILED DESCRIPTION

[0023] The following detailed description of exemplary embodiments of the present application refers to the accompanying drawings, which form a part of the description, and in which exemplary embodiments that can be implemented by the present application are shown as examples. The following more detailed description of the embodiments of the present application is not intended to limit the scope of the claimed application, but is merely for illustration and does not limit the description of the characteristics and features of the present application, so as to propose the best way to perform the application and be sufficient to enable those skilled in the art to implement the application. However, it should be understood that various modifications and variations can be made without departing from the scope of the present application as defined by the appended claims. The detailed description and drawings should be considered only as illustrative, not restrictive, and if any such modifications and variations exist, they will fall within the scope of the present application described herein. In addition, the background technology is intended to illustrate the current status and significance of the research and development of the technology and is not intended to limit the present application and the field of application of the present application.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application; the term "and / or" used herein includes any and all combinations of one or more of the relevant listed items.

[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or those recommended by the manufacturer. All reagents or instruments used, if the manufacturer is not specified, are commercially available conventional products.

[0026] To address one or more of the aforementioned technical issues, the present application provides a method for preparing a graphene micro-nanocavity TIM film, comprising at least the following steps: 1) a first coating process, wherein a graphene oxide slurry having a solid content of 3%-7% and a carbon-to-oxygen ratio of 1.2-3:1 is applied to a substrate to obtain a primary coating film, wherein the primary coating film has a coating thickness of 3-6 mm; the graphene oxide slurry is applied at a coating speed of 5-60 mm / s. Typically, but not limited to, the graphene oxide slurry coating speed is 5 mm / s, 10 mm / s, 15 mm / s, 20 mm / s, 25 mm / s, 30 mm / s, 35 mm / s, 40 mm / s, 45 mm / s, 50 mm / s, 55 mm / s, and 60 mm / s. Typically, but not limited to, the primary coating film has a coating thickness of 3 mm, 4 mm, 5 mm, and 6 mm.

[0027] A non-penetrating groove is formed by applying downward pressure along the thickness direction of the primary coating film, and a first drying process is performed to dry the primary coating film to a thickness of 40% to 75% of the pre-drying thickness. The coating thickness of the primary coating film is 3 to 6 mm. Typically, but not limited to, the coating thickness of the primary coating film is 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, 5.5 mm, and 6 mm.

[0028] The specific method for forming the grooves is to cut the primary coating film along its thickness, thereby forming a plurality of grooves spaced apart on the surface of the primary coating film. The cutting tool may be a wire, plate, or cutter, or may be a pre-set mold or machine tool. Any tool suitable for cutting grooves is applicable.

[0029] The extension direction of the groove is perpendicular to the coating direction of the primary coating film; or the extension direction of the groove is parallel to the coating direction of the primary coating film; or part of the groove is perpendicular to the coating direction of the primary coating film, and the extension direction of part of the groove is parallel to the coating direction of the primary coating film.

[0030] The width of the groove is set to 0.02mm-1mm. The spacing between the parallel and adjacent grooves is set to 0.02mm-1mm, and the spacing between adjacent grooves can be the same or different. The cutting depth of the groove is less than the thickness of the primary coating film, and the cutting depth of the groove is 10-200μm less than the thickness of the primary coating film.

[0031] The temperature of the first drying process is set at 25° C. to 65° C., and the drying time is set at 1 hour to 12 hours, and the primary coating film is dried to a thickness of 40% to 75% of the thickness before drying. Typically, but not limiting, the primary coating film is dried to a thickness of 40%, 42%, 45%, 50%, 55%, 58%, 60%, 63%, 65%, 68%, 70%, 72%, and 75% of the thickness before drying.

[0032] The second coating process involves applying the graphene oxide slurry again to the grooved surface of the primary coating film to form a secondary coating film. The secondary coating film has a thickness of 1-3 mm, with the thickness of the first coating process being greater than the thickness of the second coating process. The graphene oxide slurry is applied at a coating speed of 5-60 mm / s during the preparation of the secondary coating film. The surface of the secondary coating film remains smooth after the second coating process.

[0033] The secondary coating film is then dried a second time to obtain a graphene oxide film. During this second drying step, the drying temperature is set between 45°C and 65°C, the ambient humidity is controlled between 45% and 65% RH, and the drying time is set between 3 and 10 hours. By controlling the ambient temperature and humidity, the secondary coating film is completely dried. During the second drying process, the evaporation of water promotes the self-assembly reaction of the graphene oxide, forming a graphene oxide film with a longitudinally oriented structure.

[0034] The graphene oxide membrane is chemically foamed using a foaming agent. Hydrazine hydrate is used in this chemical foaming process. The concentration of the foaming agent is 5%-70%, the foaming temperature is 25-60°C, and the foaming time is 3-60 seconds. Preferably, the concentration is 5%-30%, and the foaming time is 3-30 seconds. The formation of bubbles of varying sizes within the graphene structure, which expand the interlayer structure of the graphene membrane and form cavities, is a key step in achieving good compressive resilience in the membrane.

[0035] The foamed graphene oxide film undergoes a thermal reduction treatment. This process includes pretreatment, carbonization, and graphitization. Pretreatment temperatures range from 170-360°C for 12-24 hours; carbonization temperatures range from 1100-1300°C for 12-17 hours; and graphitization temperatures range from 2600-3150°C for 1-2.5 hours. This thermal treatment repairs defects and reduces the chance of phonon scattering by point defects, impurities, or grain boundaries. This rearranges carbon atoms, allowing each carbon atom to form strong σ bonds with three adjacent carbon atoms through powerful sp² hybrid orbitals, enhancing the TIM film's lateral and longitudinal thermal conductivity.

[0036] The present application is further illustrated by the following examples and comparative examples.

[0037] The detection methods involved in the examples and comparative examples of this application are as follows: Compressive stress: Observe the stress change under 80% compression according to the standard "STM D575-91(2024)". The sample size is a square with a length and width of 25.4mm*25.4mm and a thickness of 1mm±0.3mm.

[0038] Longitudinal thermal conductivity: Tested according to ASTM E1461-13 Standard Test Method for Thermal Diffusivity by the Flash Method. Cut a circular sample with a diameter of 12.7 mm, measure and record the initial thickness and mass, place the sample in a test holder, and measure the thermal conductivity using a NETZSCH 467 Flash Thermal Conductivity Tester.

[0039] Example 1 1) In the first coating, a graphene oxide slurry with a solid content of 5% and a carbon-oxygen ratio of 2:1 was coated on a PP coated substrate to form a film at a coating speed of 30 mm / s to obtain a primary coating film with a coating thickness of 5 mm.

[0040] 2) Grooving: Using nylon No. 1 wire (0.18mm diameter), apply downward pressure along the thickness of the primary coating film to create non-penetrating grooves. The groove width is approximately 0.18±0.02mm, the groove depth is 4900μm, the groove opening is along the thickness direction, the groove extension direction is perpendicular to the coating direction, and the spacing between adjacent grooves is set to 0.5mm. The primary coating film with grooves enters the drying oven for the first drying process at 65°C for 1-2 hours, until the primary coating film is dried to 50% of its pre-drying thickness.

[0041] 3) A second coating process, wherein the graphene oxide slurry is again applied to the surface of the first coating film having the grooves, to obtain a second coating film. The thickness of the second coating film is 2 mm, and the thickness of the first coating process is greater than that of the second coating process. The graphene oxide slurry is applied at a coating speed of 20 mm / s during the preparation of the second coating film. The surface of the second coating film remains smooth after the second coating process.

[0042] 4) The secondary coating film is subjected to a second drying treatment to obtain a graphene oxide film; in the second drying treatment step, the drying temperature is set to 45° C., the ambient humidity is controlled at 45% RH, and the drying time is set to 8 hours.

[0043] 5) The graphene oxide film was chemically foamed using hydrazine hydrate, a foaming agent, with a mass concentration of 10%, at a foaming temperature of 45°C and a foaming time of 10 seconds.

[0044] 6) The foamed graphene oxide film was pretreated at 240°C for 17 hours, carbonized at 1200°C for 17 hours, and graphitized at 3150°C for 2 hours to obtain a graphene micro-nanocavity TIM film with a thickness of 1 mm ± 0.3 mm.

[0045] Example 2 The difference between this embodiment and embodiment 1 is that the thickness of the primary coating film obtained in the first coating process of this embodiment is 6 mm, and the thickness of the secondary coating film obtained in the second coating process is 1 mm.

[0046] 1) In the first coating, a graphene oxide slurry with a solid content of 5% and a carbon-oxygen ratio of 2:1 was coated on a PP coated substrate to form a film at a coating speed of 20 mm / s to obtain a primary coating film with a coating thickness of 6 mm.

[0047] 2) Grooving: Using nylon No. 1 wire (0.18mm diameter), apply downward pressure along the thickness of the primary coating film to create non-penetrating grooves. The groove width is approximately 0.18±0.02mm, the groove depth is 5800μm, and the groove opening is along the thickness direction. The groove extension direction and the coating direction are mutually perpendicular. The spacing between adjacent grooves is set to 1mm. The primary coating film with grooves enters the drying oven for the first drying process at 65°C for 1-2 hours, until the primary coating film is dried to 50% of its pre-drying thickness.

[0048] 3) A second coating process, wherein the graphene oxide slurry is again applied to the surface of the first coating film having the grooves, to obtain a second coating film. The thickness of the second coating film is 1 mm, and the thickness of the first coating process is greater than that of the second coating process. The graphene oxide slurry is applied at a coating speed of 60 mm / s during the preparation of the second coating film. The surface of the second coating film remains smooth after the second coating process.

[0049] 4) The secondary coating film is subjected to a second drying treatment to obtain a graphene oxide film; in the second drying treatment step, the drying temperature is set to 45° C., the ambient humidity is controlled at 45% RH, and the drying time is set to 8 hours.

[0050] 5) The graphene oxide film was chemically foamed using hydrazine hydrate, a foaming agent, with a mass concentration of 10%, at a foaming temperature of 45°C and a foaming time of 10 seconds.

[0051] 6) The foamed graphene oxide film was pretreated at 240°C for 17 hours, carbonized at 1200°C for 17 hours, and graphitized at 3150°C for 2 hours to obtain a graphene micro-nanocavity TIM film with a thickness of 1 mm ± 0.3 mm.

[0052] Example 3

[0053] The difference between this embodiment and embodiment 1 is that the thickness of the first coating film obtained in the first coating process of this embodiment is 3 mm, and the coating speed is set to 60 mm / s. The thickness of the second coating film obtained in the second coating process is 2.5 mm, and the coating speed is 5 mm / s.

[0054] Example 4 This embodiment differs from Example 1 in that a 0.5 mm thick acrylic plate is used as a cutting die. Downward pressure is applied to the primary coating film to produce non-penetrating grooves. The groove width is 0.5 ± 0.02 mm, and the spacing between adjacent parallel grooves is set to 1 mm. The cutting depth of the grooves is set to 4900 μm.

[0055] 1) In the first coating, a graphene oxide slurry with a solid content of 5% and a carbon-oxygen ratio of X was coated on a PP coated substrate to form a film at a coating speed of 30 mm / s to obtain a primary coating film with a coating thickness of 5 mm.

[0056] 2) Create grooves: A 0.5mm-thick acrylic sheet is used as a cutting die. Downward pressure is applied along the thickness of the primary coating film to create non-penetrating grooves. The groove width is approximately 0.5±0.02mm, the depth is 200μm, and the groove opening is along the thickness direction, with the groove extending perpendicular to the coating direction. The primary coating film with grooves is placed in a drying oven for the first drying process at 65°C for 1-2 hours, until the primary coating film is dried to 50% of its pre-drying thickness.

[0057] 3) A second coating process, wherein the graphene oxide slurry is again applied to the surface of the first coating film having the grooves, to obtain a second coating film. The thickness of the second coating film is 2 mm, and the thickness of the first coating process is greater than that of the second coating process. The graphene oxide slurry is applied at a coating speed of 20 mm / s during the preparation of the second coating film. The surface of the second coating film remains smooth after the second coating process.

[0058] 4) The secondary coating film is subjected to a second drying treatment to obtain a graphene oxide film; in the second drying treatment step, the drying temperature is set to 45° C., the ambient humidity is controlled at 45% RHRH, and the drying time is set to 8 hours.

[0059] 5) The graphene oxide film was chemically foamed using hydrazine hydrate, a foaming agent, with a mass concentration of 10%, at a foaming temperature of 45°C and a foaming time of 10 seconds.

[0060] 6) The foamed graphene oxide film was pretreated at 240°C for 17 hours, carbonized at 1200°C for 17 hours, and graphitized at 3150°C for 2 hours to obtain a graphene micro-nanocavity TIM film with a thickness of 1 mm ± 0.3 mm.

[0061] Example 5 The difference between this embodiment and embodiment 1 is that the spacing between the parallel and adjacent grooves is set to 0.20±0.02 mm.

[0062] Example 6 The difference between this embodiment and embodiment 1 is that the spacing between the parallel and adjacent grooves is set to 1±0.02 mm.

[0063] The graphene micro-nanocavity TIM films obtained in Examples 1 to 6 were subjected to longitudinal thermal conductivity tests. The test results are shown in the following table:

[0064] From the test results, it was found that the longitudinal thermal conductivity of the graphene TIM films obtained by the process method of the present invention in Examples 1-6 was greater than 15W / mK, which is 3-5 times that of conventional graphene micro-nanocavity thermal conductive films, and has higher longitudinal heat transfer performance. The first coating thickness of Example 1 is 5mm, and the longitudinal thermal conductivity is 19.2W / mK. The first coating thickness in Example 2 is 6mm, which is an improvement over the longitudinal thermal conductivity of Example 1, and the longitudinal thermal conductivity can reach 21.3W / mK. The first coating thickness of Example 3 is 3mm, which is thinner than that of Examples 1 and 2, and the longitudinal thermal conductivity is 17.1W / mK. From the test results of Examples 1-3, it can be seen that changing the first coating thickness has an impact on the longitudinal thermal conductivity of the graphene TIM film. The thicker the first coating thickness, the more obvious the improvement in the longitudinal thermal conductivity. This is because the thicker the first coating thickness is, the more space there is to guide the graphene oxide microsheets to be oriented along the thickness direction when applying downward pressure during groove formation, and the more obvious the improvement in longitudinal thermal conductivity is.

[0065] Example 4 varied the groove width to explore the effect of this change on the longitudinal thermal conductivity of the graphene TIM film. The longitudinal thermal conductivity of Example 4 was measured to be 16.4 W / mK. This represents a decrease in longitudinal thermal conductivity compared to Example 1. Analysis suggests that increasing the groove width reduces the number of grooves per unit area, naturally reducing the number of longitudinal thermal paths created. Therefore, the improvement in longitudinal thermal conductivity achieved in Example 4 is diminished, resulting in overall inferior longitudinal thermal conductivity compared to Example 1.

[0066] Examples 5 and 6 changed the spacing of the grooves to explore the effect of the change in groove spacing on the improvement of the longitudinal thermal conductivity of the graphene TIM film. The groove spacing of Example 5 is tighter than that of Example 1, and the longitudinal thermal conductivity is 23.6W / mK, which is significantly improved compared to Example 1. The groove spacing of Example 6 is looser than that of Example 1, and the longitudinal thermal conductivity is 15.3W / mK. After analysis, it is believed that the improvement in the longitudinal thermal conductivity is proportional to the number of grooves per unit area. The more grooves are set per unit area, the more help is provided for the construction of the longitudinally arranged heat conduction channel of graphene. Therefore, the longitudinal thermal conductivity of the graphene TIM film is further improved.

[0067] For the graphene TIM films prepared by the methods of Examples 1-6, the transient compressive stress at 80% compression was ≤110 psi, and the static compressive stress at 80% compression was ≤50 psi. Furthermore, test data revealed that the compressive stress is related to the initial coating thickness: as the initial coating thickness decreases, the static and transient compressive stresses also decrease. Figure 6This is a compression property test of Example 2. The actual thickness of the sample of Example 2 is 1.1 mm. Pressure is continuously applied to the sample. When the TIM film of Example 2 is compressed 80%, the transient force is 470.75 N and the static force is 219.93 N. After conversion, it is found that the transient compressive stress is 105.8 PSI and the static compressive stress is 49.4 PSI.

[0068] It should be noted that the ratio of raw materials and the preparation process not mentioned above can all be referred to the existing technology and will not be described in detail here.

[0069] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0070] Although the present application has been shown and described with reference to certain preferred embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the application.

Claims

1. A method for manufacturing a graphene micro-nanocavity TIM film, characterized by: At least the following steps are included: 1) A first coating process is performed by coating a graphene oxide slurry on a substrate to obtain a primary coating film; 2) a downward pressure is applied along the thickness direction of the primary coating film to form a non-penetrating groove, and a first drying process is performed to dry the primary coating film until its thickness is 40%-75% of that before drying; 3) a second coating process is performed by coating the graphene oxide slurry again on the surface of the primary coating film with the groove to obtain a secondary coating film, wherein the thickness of the primary coating film is greater than that of the secondary coating film; 4) a second drying process is performed on the secondary coating film to obtain a graphene oxide film; 5) the graphene oxide film is foamed and heat-treated in sequence to obtain a graphene micro-nanocavity TIM film.

2. The method for preparing a graphene micro-nanocavity TIM film according to claim 1, characterized in that: The specific method of manufacturing the grooves is to cut the primary coating film along the thickness direction to form a plurality of grooves arranged at intervals on the surface of the primary coating film.

3. The method for preparing a graphene micro-nanocavity TIM film according to claim 2, characterized in that: The extension direction of the groove is perpendicular to the coating direction of the primary coating film; or the extension direction of the groove is parallel to the coating direction of the primary coating film; or part of the groove is perpendicular to the coating direction of the primary coating film, and the extension direction of part of the groove is parallel to the coating direction of the primary coating film.

4. The method for preparing a graphene micro-nanocavity TIM film according to claim 3, characterized in that: The width of the groove is set to 0.02mm-1mm.

5. The method for preparing a graphene micro-nanocavity TIM film according to claim 3, characterized in that: The spacing between the parallel and adjacent grooves is set to 0.02mm-1mm, and the spacing between the adjacent grooves is the same or different.

6. The method for preparing a graphene micro-nanocavity TIM film according to claim 3, characterized in that: The cutting depth of the groove is smaller than the thickness of the primary coating film, and the cutting depth of the groove is 10-200 μm less than the thickness of the primary coating film.

7. The method for preparing a graphene micro-nanocavity TIM film according to claim 1, characterized in that: The solid content of the graphene oxide slurry is 3%-7%, and the carbon-oxygen ratio is 1.2-3:

1.

8. The method for preparing a graphene micro-nanocavity TIM film according to claim 1, characterized in that: When preparing the first coating film, the coating speed of the graphene oxide slurry is 5-60 mm / s, preferably, the coating speed is 10-40 mm / s.

9. The method for preparing a graphene micro-nanocavity TIM film according to claim 1, characterized in that: The thickness of the first coating is greater than the thickness of the second coating.

10. A graphene micro-nanocavity TIM film, characterized by: The graphene micro-nano cavity TIM film is obtained by the preparation method according to claims 1-7; the density of the graphene micro-nano cavity TIM film is ≥0.1g / cm 3 , thickness is 1mm±0.3mm, transient compressive stress at 80% compression is ≤110psi, static compressive stress at 80% compression is ≤50Psi, longitudinal thermal conductivity is ≥15W / (mK), preferably, longitudinal thermal conductivity is ≥20W / (mK).