Separation method and content determination method of titanium foreign matter in lithium battery positive electrode material

By employing a method involving sodium hexametaphosphate dispersant sieving, concentrated nitric acid passivation, hydrochloric acid oxidation-reduction, and ammonium bifluoride digestion, the problem of accurate separation and detection of titanium foreign matter in lithium battery cathode materials was solved. This method ensured the original morphology and content determination of titanium foreign matter, optimized sample pretreatment, improved detection accuracy, and reduced costs.

CN120820398AActive Publication Date: 2025-10-21XTC NEW ENERGY MATERIALS (NINGDE) CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202511329939.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-17
Publication Date
2025-10-21
Estimated Expiration
2045-09-17

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively separate and accurately measure titanium foreign matter in lithium-ion battery cathode materials. In particular, titanium particles are non-magnetic and easily mix with other particles, resulting in low detection accuracy. Furthermore, traditional methods may alter the chemical morphology of titanium foreign matter or lead to content loss.

Method used

A dense oxide film was formed to protect the titanium surface by using sodium hexametaphosphate dispersant sieving, concentrated nitric acid passivation, hydrochloric acid redox reaction and ammonium bifluoride digestion. Combined with ICP testing, it was ensured that the titanium foreign matter was not digested and retained its original morphology, thus optimizing the sample pretreatment steps.

Benefits of technology

This method enables accurate separation and content determination of titanium foreign matter in lithium battery cathode materials, reducing complex operation steps and the consumption of expensive reagents, and improving the accuracy and reliability of detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120820398A_ABST
    Figure CN120820398A_ABST
Patent Text Reader

Abstract

The invention provides a separation method and a content determination method for titanium foreign matters in a lithium battery positive electrode material, through the step design of material screening, metal titanium particle purification, metal titanium particle digestion and titanium content determination, and by means of a specific mixed acid system, the digestion process is accurately controlled, the positive electrode material is effectively digested, and meanwhile, the titanium foreign matters in the lithium battery positive electrode material are effectively separated. Through the early-stage passivation process, a layer of compact oxidation film with titanium dioxide as the main component can be rapidly formed on the titanium surface, internal titanium is effectively prevented from continuously reacting with nitric acid and hydrochloric acid, and the original form and content of the metallic titanium foreign matter are reserved to the maximum extent; therefore, the content of the titanium foreign matters in the material is accurately measured, and meanwhile, by optimizing a sample pretreatment mode, complex and high-cost operation steps are reduced, and consumption of expensive reagents is reduced. The invention provides a new detection thought and method, fills the blank in the related technical field, and promotes the development and application of the detection technology in the field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium batteries, and in particular to a method for separating titanium foreign matter from a positive electrode material of a lithium battery and a method for determining its content. Background Art

[0002] Magnetic particles are becoming a key safety indicator in the testing of lithium battery cathode materials. The primary source of magnetic particles is friction between materials and stainless steel components in production equipment. To reduce the introduction of magnetic particles, titanium components are increasingly used in production equipment. However, with long-term continuous operation, equipment inevitably experiences normal wear and tear. This wear can cause titanium to dislodge from the equipment as tiny particles and mix into the material being processed, exposing the material to the risk of contamination.

[0003] Patent CN 115290416 A provides a magnetic particle cleanliness test method that fully extracts magnetic particles from particles adsorbed by a magnetic rod wrapped in a thermoplastic bag. However, this method only detects magnetic particulate foreign matter. Metal Ti particles are not magnetic and cannot be separated by magnetic separation.

[0004] Patent CN 118437052 A provides a rapid screening device and screening method for small-particle cathode material. It can quickly screen the particles, but in actual application, the screened material will contain agglomerated cathodes, alumina debris, etc., accounting for between 80-95%. As a result, titanium particles are a small amount of elements and cannot be quickly detected by energy spectrum. Even if they are completely digested in ICP testing, there is interference from the matrix, which is not conducive to detection.

[0005] Patent CN 117629974 A provides a method for determining aluminum and zirconium in cathode materials. This method employs a mixed acid digestion method that can completely digest the cathode sample, eliminating insoluble matter from the digestion product and improving the accuracy of the test results. However, this method cannot eliminate the aqueous filter membrane after filtration, and membrane residue may clog the sample injection system during volume determination.

[0006] Patent CN 117269154 A provides a method for detecting metallic impurities in electrolytes, including an inorganic acid digestion solution. This solution dissolves metallic impurities in the form of solid particles, leaving them in the test solution as cations for quantitative measurement. However, this solution is ineffective in dissolving titanium particles, as an oxide film forms on the titanium surface, which the inorganic acid digestion system struggles to break.

[0007] Currently, the main methods for detecting metal particles include cleanliness testing, energy spectrum testing, and ICP testing. Since titanium is non-magnetic, it cannot be separated by magnetic separation, and screening is the only method. However, even after screening, titanium foreign matter may still be mixed with larger particles of material. These larger particles mainly come from material agglomeration and alumina particles in production tooling, making it difficult to accurately distinguish titanium particles, resulting in low test accuracy. Summary of the Invention

[0008] The present application is made in view of the above-mentioned issues, and its purpose is to provide a method for effectively digesting the positive electrode material while ensuring that the metal titanium foreign matter is not digested, so as to retain the original form and content of the metal titanium foreign matter to the greatest extent, and at the same time eliminate the influence of the sample matrix composition on the test results, thereby realizing a method for separating titanium foreign matter in the material and a method for accurately determining its content.

[0009] In order to achieve the above object, the present application provides a method for separating titanium foreign matter from a lithium battery positive electrode material, comprising the following steps: 1) Sample screening: Weigh the material, add sodium hexametaphosphate dispersant, place it on a roller mill to fully mix the material and dispersant, use a sieve to screen, then rinse the remaining material on the sieve into a beaker, and then filter the solution in the beaker to obtain the pre-treated material; 2) Passivation process: Add concentrated nitric acid to the pre-treatment material and stir at room temperature for a period of time; 3) Material impurity removal: In a water bath environment, hydrochloric acid is added to the passivated material and stirred to cause a redox reaction to digest the positive electrode material. After the reaction is completed, titanium metal particles are obtained by filtration; 4) Ti particle digestion: Add ammonium bifluoride and aqua regia to the filter membrane and titanium metal particles after filtration in step 3), place on a 150-250°C hot plate and digest for 15-60 minutes to obtain soluble hexafluorotitanate complex ions.

[0010] In any embodiment, in step 1), 5-10% by weight of the material of sodium hexametaphosphate dispersant is added; the sodium hexametaphosphate is completely dissolved in pure water with a concentration of 1-2%.

[0011] In any embodiment, in step 1), the material and dispersant are placed above the roller of a roller mill, and are processed by the roller at 55-65 r / min for 25-40 min to fully mix the material and dispersant, and then screened using a mat-type screen.

[0012] In any embodiment, the screen is a mat-type screen with an area size of D60 mm and an aperture of 500-800 mesh.

[0013] In any embodiment, the ratio of concentrated nitric acid added in step 2) to the material is 5-10 mL: 1 kg, and the reaction time is 5-10 min.

[0014] In any embodiment, the ratio of hydrochloric acid added in step 3) to the material is 5-10 mL: 1 kg.

[0015] In any embodiment, in step 3), the water bath reaction temperature is 50-90° C., and the reaction time is 20-30 min.

[0016] In any embodiment, the concentration of concentrated nitric acid is 65% to 70%, and the concentration of hydrochloric acid is 36% to 38%; in step 4), the ratio of ammonium bifluoride to material is 1-2 g:1 kg, and the ratio of aqua regia to material is 8-16 mL:1 kg.

[0017] In any embodiment, the stirring in steps 2) and 3) is magnetic stirring, and the stirring speed is 300-600 r / min.

[0018] A method for determining the content of titanium foreign matter in a lithium battery positive electrode material comprises cooling the solution obtained by the above separation method, fixing the volume, and performing an ICP test to obtain the content of titanium foreign matter in the lithium battery positive electrode material.

[0019] Beneficial effects of this application: The present invention focuses on the method of purifying and determining metallic titanium particles. Through the design of the steps of material screening-purification of metallic titanium particles-digestion of metallic titanium particles-determination of titanium content, with the help of a specific mixed acid system, the digestion process is accurately controlled. While effectively digesting the positive electrode material, it ensures that metallic titanium foreign matter is not digested. Through the early passivation process, a dense oxide film with titanium dioxide as the main component will quickly form on the titanium surface. The oxide film can effectively prevent the internal titanium from continuing to react with nitric acid and hydrochloric acid, retaining the original form and content of metallic titanium foreign matter to the greatest extent, avoiding the chemical form change and content loss of titanium foreign matter caused by traditional pretreatment methods, and eliminating the influence of the sample matrix component on the test results, thereby achieving accurate determination of the titanium foreign matter content in the material. At the same time, by optimizing the sample pretreatment method, the complex and high-cost operation steps are reduced, and the consumption of expensive reagents is reduced. The present invention provides a new detection idea and method, filling the gap in the relevant technical field, and promoting the development and application of detection technology in this field. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a comparison chart of the digestion of the positive electrode material in the control experiment with different pretreatment stirring times set in Example 2. DETAILED DESCRIPTION

[0021] Below, with appropriate reference to the accompanying drawings, the embodiments of the method for separating titanium foreign matter and the method for determining its content in the positive electrode material of a lithium battery of the present application are described in detail. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0022] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0023] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0024] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0025] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0026] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0027] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0028] The present invention utilizes a specific mixed acid system to precisely control the digestion process, effectively digesting the positive electrode material while ensuring that metallic titanium foreign matter is not digested. This not only maximizes the preservation of the original form and content of metallic titanium foreign matter, but also completely digests the aqueous filter membrane (to obtain the oversize material, the material must be filtered after sieving) without leaving any residue, thus avoiding the problems of traditional pretreatment methods: traditional methods can cause the chemical form of metallic titanium foreign matter to change and its content to be lost. Because the filter membrane may retain material, it must be treated during digestion. During the digestion process, the filter membrane forms residues that remain in the beaker. During subsequent sample volume testing, these filter membrane residues enter the ICP liquid inlet tube, interfering with and clogging the sample injection system, affecting the accurate determination of the metallic titanium foreign matter content in the material. As a result, the present invention achieves accurate determination of the metallic titanium foreign matter content in the material. At the same time, by optimizing the sample pretreatment method, complex and costly operational steps are reduced, reducing the consumption of expensive reagents. In terms of filling technical gaps, given that the existing ICP technology for detecting titanium foreign matter has many shortcomings and there is currently a lack of effective methods for determining the content of titanium foreign matter in lithium battery positive electrode materials, the present invention provides a new detection idea and method, filling the gap in the relevant technical field and promoting the development and application of detection technology in this field.

[0029] In one embodiment of the present application, the present application proposes a method for separating titanium foreign matter in a lithium battery positive electrode material, comprising the following steps: 1) Sample screening: Weigh the material, add sodium hexametaphosphate dispersant, place it on a roller mill to fully mix the material and dispersant, use a sieve to screen, then rinse the remaining material on the sieve into a beaker, and then filter the solution in the beaker to obtain the pre-treated material; The material that needs to be separated and tested in the lithium battery positive electrode material of this application is the content of impurity titanium particles mixed in due to mechanical wear. The content of such impurity titanium particles in the material is relatively low, and a small amount of titanium particles may be mixed in several tons of material. Therefore, the amount of material required in the pretreatment stage must be at least 1 kg to ensure that there is a sufficient probability to capture the target impurities. This 1 kg of material cannot be completely digested with acid. The material and titanium particles must be sieved and separated first. The role of sodium hexametaphosphate is to improve the dispersion and fluidity of the material, allowing the material to pass through the screen more smoothly, thereby improving the separation efficiency of titanium particles and materials. The material after screening is usually less than 1g, and this part of the material is then digested.

[0030] 2) Passivation process: Add concentrated nitric acid to the pre-treated material (screened material) and stir at room temperature for a period of time; At room temperature, a dense oxide film with titanium dioxide (TiO2) as the main component will quickly form on the surface of titanium. This oxide film can effectively prevent the internal titanium from continuing to react with nitric acid and hydrochloric acid.

[0031] 3) Material impurity removal: In a water bath environment, hydrochloric acid is added to the passivated material and stirred to cause a redox reaction to digest the positive electrode material. After the reaction is completed, titanium metal particles are obtained by filtration; The main components of the positive electrode material will react with the chloride ions (Cl - ) undergoes an oxidation-reduction reaction, thereby achieving the digestion of the positive electrode material. After the reaction is completed, metallic titanium (Ti) particles can be obtained by filtration.

[0032] 4) Ti particle digestion: ammonium bifluoride and aqua regia are added to the filter membrane and titanium metal particles after filtration in step 3) to obtain soluble hexafluorotitanate complex ions.

[0033] Ammonium bifluoride reacts with nitric acid, which, as a strong acid, dissociates into hydrogen ions (H + ), which can inhibit the fluoride ion (F - ) hydrolyzes, thereby providing free F for the reaction - , F - It can react with TiO2 on the titanium surface to generate soluble hexafluorotitanate complex ions.

[0034] In any embodiment, in step 1), 5-10% by weight of the material of sodium hexametaphosphate dispersant is added; the sodium hexametaphosphate is completely dissolved in pure water with a concentration of 1-2%.

[0035] If the concentration is too low, the dispersion effect is poor and the material screening speed is slow. If the concentration is too high, the sodium hexametaphosphate particles will aggregate and dissolve slowly, requiring high temperature dissolution, which is costly.

[0036] In any embodiment, in step 1), the material and dispersant are placed above the roller of a roller mill, and are processed by the roller at 55-65 r / min for 25-40 min to fully mix the material and dispersant, and then screened using a mat-type screen.

[0037] Roller processing time is too short: material mixing is not sufficient; time is too long: efficiency is wasted, materials that do not need to be processed for a long time; speed is too low: mixing is uneven; speed is too fast: increase wear and affect equipment efficiency. The material and dispersant can be fully mixed.

[0038] In any embodiment, the screen is a mat-type screen with an area size of D60 mm and an aperture of 500-800 mesh.

[0039] The mat-type screen has a small area, which makes the collection of the screen material fast and efficient, and can achieve the effect of complete collection.

[0040] In any embodiment, the ratio of concentrated nitric acid added in step 2) to the material is 5-10 mL: 1 kg, and the reaction time is 5-10 min.

[0041] Excessive dosage: waste of resources, excess nitric acid does not participate in the formation of oxide film, TiO2 does not react with concentrated nitric acid after stabilization, only increases costs and increases safety risks, too little dosage: incomplete oxide film, only a thin oxide film is formed locally on the titanium surface, and there are a large number of exposed active sites, too low concentration: dilute nitric acid has weak oxidizing ability, cannot quickly oxidize Ti and form a dense oxide film, and the protective property of the film layer fails, the reaction time is too short: the oxidation reaction is not completed, and the TiO2 film only covers part of the active sites, the reaction time is too long: extending the time will not make the film layer denser, but will cause side reactions.

[0042] In any embodiment, the ratio of hydrochloric acid added in step 3) to the material is 5-10 mL: 1 kg.

[0043] Too little dosage: the cathode material is not completely digested, and unreacted cathode particles remain in the solution. Too much dosage: increase costs and increase safety risks. - The reducing property is weak, the driving force of the redox reaction is insufficient, and the reaction time is prolonged.

[0044] In any embodiment, in step 3), the water bath reaction temperature is 50-90° C., and the reaction time is 20-30 min.

[0045] If the reaction temperature is too low, the nickel, cobalt, and manganese metal elements in the cathode material will be difficult to completely dissolve, resulting in a large number of undigested solid particles remaining in the solution. At the same time, the digestion solution will not react completely and will be consumed slowly, which will extend the overall processing cycle. If the temperature is too high, the digestion solution will evaporate violently, causing the acid concentration in the system to drop rapidly, which will inhibit the digestion reaction. When the amount of acid is insufficient, the dissolution rate of the cathode material will decrease. In addition, high temperature may partially dissolve the originally stable titanium particles, affecting the accuracy of the detection.

[0046] If the reaction time is too short, the digestion is incomplete and a large amount of positive electrode material particles remain. If the reaction time is too long, the hydrochloric acid evaporates excessively and energy consumption increases.

[0047] In any embodiment, in step 4), the ratio of ammonium bifluoride to material is 1-2 g:1 kg, and the ratio of aqua regia to material is 8-16 mL:1 kg.

[0048] Too little dosage: F - Insufficient, TiO2 on the titanium surface cannot be completely converted into [TiF6] 2- , residual oxide film, excessive use: increase cost, increase safety risk. Concentration is too low: cannot inhibit F - Hydrolysis, effective F - If the concentration decreases, the reaction time is too short: digestion is incomplete; if the reaction time is too long: energy consumption increases.

[0049] In any embodiment, the stirring in steps 2) and 3) is magnetic stirring at a stirring speed of 300-600 r / min. Magnetic stirring is efficient and stable, allowing the material and the reagent to react fully.

[0050] When the stirring rate is too low, the magnet rotates slowly and cannot fully drive the flow of the digestion solution, resulting in uneven mixing of the system and large differences in local acid concentration. The positive electrode material particles are prone to sedimentation and aggregation, making it difficult for them to fully contact the digestion solution, resulting in incomplete digestion. If the stirring rate is too high, high-speed stirring will cause the digestion solution to churn violently, even splashing out of the container, resulting in material loss, and causing the acid concentration to drop, affecting the digestion effect.

[0051] In addition, the present application also provides a method for determining the content of titanium foreign matter in the positive electrode material of a lithium battery. The solution obtained by the separation method is cooled and then fixed to a constant volume, and an ICP test is performed to obtain the content of titanium foreign matter in the positive electrode material of the lithium battery.

[0052] Example Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0053] Example 1 A method for separating and determining the content of titanium foreign matter in a lithium battery positive electrode material comprises the following steps: 1. Weigh 1kg of the sample to be tested, add 2% sodium hexametaphosphate solution, shake evenly, and place on a roller mill. Set the roller parameters to: 30 minutes, 60 rpm, to fully mix the material and dispersant. Sieve using a mat-type screen. Rinse the remaining material on the screen into a beaker, and then filter the solution in the beaker.

[0054] 2. After filtration, place a magnet in the beaker, add 10 mL of nitric acid, stir at room temperature for 10 minutes, then add 10 mL of hydrochloric acid, place in a 50°C water bath and stir for 30 minutes. After stirring, filter the material in the beaker.

[0055] 3. Place the filter membrane in a polytetrafluoroethylene beaker. Add 2g of ammonium bifluoride, 6mL of hydrochloric acid, and 2mL of nitric acid. Digest the membrane on a 200°C hot plate for 15-60 minutes. After digestion, remove the membrane from the beaker, cool it, and then adjust the volume.

[0056] 4. After sample pretreatment is completed, turn on the inductively coupled plasma optical emission spectrometer (ICP-OES) according to the instrument operating procedures. After the equipment is preheated and stabilized, the torch flame is ignited normally, and all parameters (RF power, nebulizing gas flow rate, auxiliary gas flow rate, etc.) reach the set standards, use the ICP equipment to perform quantitative testing on the test solution that has been diluted to 50 mL.

[0057]

[0058] Through the comparison of data from the control experiments with different digestion times (15 min, 30 min, 45 min, 60 min) set in Example 1, it can be seen that under the same mixed acid system (ammonium bifluoride, concentrated nitric acid and hydrochloric acid), water bath temperature and stirring rate, when the digestion time is controlled to 45 min, the digestion effect of titanium (Ti) particles is significantly better than that of other groups. At this time, the titanium dioxide (TiO2) oxide film on the surface of the Ti particles is replaced by free fluoride ions (F - ) fully penetrates, and the generated soluble hexafluorotitanate complex ion ([TiF6] 2-) are evenly dispersed in the solution. Combining various data and phenomena, it can be seen that a digestion time of 45 minutes can achieve more thorough digestion of Ti particles. Within the conditions set in this set of experiments, it is a parameter that is more conducive to achieving efficient and deep digestion of Ti particles.

[0059] Example 2 A method for separating and determining the content of titanium foreign matter in a lithium battery positive electrode material comprises the following steps: 1. Weigh 1 kg of the sample to be tested, add 2% sodium hexametaphosphate solution, shake well, and place on a roller mill. Set the roller parameters to: 30 minutes, 60 rpm to thoroughly mix the material and dispersant. Sieve using a mat-type screen. Rinse any remaining material on the screen into a beaker, then filter the solution.

[0060] 2. After filtration, place a magnet in the beaker, add 10 mL of nitric acid, stir at room temperature for 10 minutes, then add 10 mL of hydrochloric acid, place in a 50°C water bath and stir for 10-30 minutes. After stirring, filter the material in the beaker.

[0061] 3. Place the filter membrane in a polytetrafluoroethylene beaker. Add 2g of ammonium bifluoride, 6mL of hydrochloric acid, and 2mL of nitric acid. Digest on a 200°C hot plate for 45 minutes. After digestion, remove the membrane and cool it down to a constant volume.

[0062] 4. After sample pretreatment is completed, turn on the inductively coupled plasma optical emission spectrometer (ICP-OES) according to the instrument operating procedures. After the equipment is preheated and stabilized, the torch flame is ignited normally, and all parameters (RF power, nebulizing gas flow rate, auxiliary gas flow rate, etc.) reach the set standards, use the ICP equipment to perform quantitative testing on the test solution that has been diluted to 50 mL.

[0063] A comprehensive data comparison of multiple groups of experiments with different pretreatment stirring times (10 min, 20 min, 30 min) set in Example 2 was conducted and it was found that (eg Figure 1 ): Under the same mixed acid system (ammonium bifluoride, concentrated nitric acid and hydrochloric acid), water bath temperature and stirring rate conditions, when the pretreatment stirring time is controlled at 30 minutes, the main components of the positive electrode material will react with the chloride ions (Cl - ) undergoes redox reaction, and the reaction time is more sufficient, thereby achieving the digestion of the positive electrode material. After the reaction is completed, metallic titanium (Ti) particles can be obtained by filtration. Since the positive electrode material is eliminated more thoroughly, the test interference is reduced, making the subsequent Ti particle content test more efficient and accurate.

[0064] Example 3 A method for separating and determining the content of titanium foreign matter in a lithium battery positive electrode material comprises the following steps: 1. Weigh 1 kg of the sample to be tested, add 2% sodium hexametaphosphate solution, shake well, and place on a roller mill. Set the roller parameters to: 30 minutes, 60 rpm to thoroughly mix the material and dispersant. Sieve using a mat-type screen. Rinse any remaining material on the screen into a beaker, then filter the solution.

[0065] 2. After filtration, place a magnet in the beaker, add 0-10 mL of nitric acid, stir at room temperature for 10 minutes, then add 10 mL of hydrochloric acid, place in a 50°C water bath and stir for 30 minutes. After stirring, filter the material in the beaker.

[0066] 3. Place the filter membrane in a polytetrafluoroethylene beaker. Add 2g of ammonium bifluoride, 6mL of hydrochloric acid, and 2mL of nitric acid. Digest on a 200°C hot plate for 45 minutes. After digestion, remove the membrane and cool it down to a constant volume.

[0067] 4. After sample pretreatment is completed, turn on the inductively coupled plasma optical emission spectrometer (ICP-OES) according to the instrument operating procedures. After the equipment is preheated and stabilized, the torch flame is ignited normally, and all parameters (RF power, nebulizing gas flow rate, auxiliary gas flow rate, etc.) reach the set standards, use the ICP equipment to perform quantitative testing on the test solution that has been diluted to 50 mL.

[0068]

[0069] After comparative analysis of multiple groups of experiments with different nitric acid contents (0 mL, 5 mL, 10 mL, and 20 mL) pretreatments set in Example 3, it was found that under the conditions of the same mixed acid system (ammonium bifluoride, concentrated nitric acid, and hydrochloric acid) and consistent water bath temperature and stirring rate, nitric acid, due to its strong oxidizing property, drives a rapid oxidation reaction on the surface of the titanium particles, promoting the efficient combination of titanium (Ti) and oxygen to form a dense and uniform titanium dioxide (TiO2) passivation film. When the nitric acid content is 10 mL, the integrity, density, and stability of the passivation film on the titanium particle surface are optimized. The titanium particles pretreated in this way can prevent further reaction with hydrochloric acid during the subsequent pretreatment stirring process, providing a guarantee for the accuracy of the subsequent titanium particle content measurement.

[0070] Example 4 A method for separating and determining the content of titanium foreign matter in a lithium battery positive electrode material comprises the following steps: 1. Weigh 1 kg of the sample to be tested, add 2% sodium hexametaphosphate solution, shake well, and place on a roller mill. Set the roller parameters to: 30 minutes, 60 rpm to thoroughly mix the material and dispersant. Sieve using a mat-type screen. Rinse any remaining material on the screen into a beaker, then filter the solution.

[0071] 2. After filtration, place a magnet in the beaker, add 10 mL of nitric acid, stir at room temperature for 10 minutes, then add 10 mL of hydrochloric acid, place in a 50°C water bath and stir for 30 minutes. After stirring, filter the material in the beaker.

[0072] 3. Place the filter membrane in a polytetrafluoroethylene beaker. Add 2g of ammonium bifluoride, 6mL of hydrochloric acid, and 2mL of nitric acid. Digest on a hot plate at 100-200°C for 45 minutes. After digestion, remove the membrane and cool it down to a constant volume.

[0073] 4. After sample pretreatment is completed, turn on the inductively coupled plasma optical emission spectrometer (ICP-OES) according to the instrument operating procedures. After the equipment is preheated and stabilized, the torch flame is ignited normally, and all parameters (RF power, nebulizing gas flow rate, auxiliary gas flow rate, etc.) reach the set standards, use the ICP equipment to perform quantitative testing on the test solution that has been diluted to 50 mL.

[0074]

[0075] Comparison and analysis of multiple experimental data sets at different digestion temperatures (100°C, 150°C, 200°C, and 250°C) in Example 4 clearly demonstrate that, under the same mixed acid system (ammonium bifluoride, concentrated nitric acid, and hydrochloric acid), water bath temperature, and stirring rate, the digestion effect of Ti particles at 200°C is significantly superior to that at other temperature groups. The Ti content percentage data at this temperature demonstrates outstanding performance. Compared with temperature groups such as 100°C and 150°C, Ti particles are digested to a higher degree and with less residue, achieving more efficient Ti particle digestion. Higher temperature groups, such as 250°C, may induce side reactions or reduce system stability due to excessively high temperatures, thus affecting the digestion effect. Comprehensive analysis of these data and phenomena indicates that a digestion temperature of 200°C results in more thorough Ti particle digestion and, within the experimental conditions set, is the temperature parameter most conducive to efficient and deep Ti particle digestion.

[0076] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A method for separating titanium foreign matter from a lithium battery positive electrode material, characterized in that: The following steps are involved: 1) Sample screening: Weigh the material, add sodium hexametaphosphate dispersant, place it on a roller mill to fully mix the material and dispersant, use a sieve to screen, then rinse the remaining material on the sieve into a beaker, and then filter the solution in the beaker to obtain the pre-treated material; 2) Passivation process: Add concentrated nitric acid to the pre-treatment material and stir at room temperature for a period of time; 3) Material impurity removal: In a water bath environment, hydrochloric acid is added to the passivated material and stirred to cause a redox reaction to digest the positive electrode material. After the reaction is completed, titanium metal particles are obtained by filtration; 4) Ti particle digestion: Add ammonium bifluoride and aqua regia to the filter membrane and titanium metal particles after filtration in step 3), place on a 150-250°C hot plate and digest for 15-60 minutes to obtain soluble hexafluorotitanate complex ions.

2. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1, characterized in that: In step 1), 5-10% of the weight of the material is added as a sodium hexametaphosphate dispersant; the sodium hexametaphosphate is completely dissolved in pure water with a concentration of 1-2%.

3. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1, characterized in that: In step 1), the material and dispersant are placed above the roller of the roller mill and processed at 55-65 r / min for 25-40 minutes to fully mix the material and dispersant, and then screened using a mat-type screen.

4. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1 or 3, characterized in that: The screen is a mat-type screen with an area size of D60mm and an aperture of 500-800 meshes.

5. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1, characterized in that: The ratio of concentrated nitric acid added in step 2) to the material is 5-10 mL: 1 kg, and the reaction time is 5-10 min.

6. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1, characterized in that: The ratio of hydrochloric acid added in step 3) to the material is 5-10 mL: 1 kg.

7. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1, characterized in that: In step 3), the water bath reaction temperature is 50-90° C., and the reaction time is 20-30 min.

8. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1 or 5, characterized in that: The concentration of the concentrated nitric acid is 65% to 70%, and the concentration of the hydrochloric acid is 36% to 38%. In step 4), the ratio of ammonium bifluoride to the material is 1-2 g:1 kg, and the ratio of aqua regia to the material is 8-16 mL:1 kg.

9. The method for separating titanium foreign matter from a lithium battery positive electrode material according to claim 1, characterized in that: The stirring in steps 2) and 3) is magnetic stirring, and the stirring speed is 300-600 r / min.

10. A method for determining the content of titanium foreign matter in a lithium battery positive electrode material, characterized in that: The solution obtained by the separation method according to any one of claims 1 to 9 is cooled and then constant in volume, and an ICP test is performed to obtain the content of titanium foreign matter in the lithium battery positive electrode material.

Citation Information

Patent Citations

  • Magnetic particle cleanliness testing method

    CN115290416A

  • Application method of ammonium bifluoride as geological sample digestion reagent

    CN102854053A

  • Producing a titanium product

    CN105658582A

  • Anti-alkali metal poisoning denitration catalyst, preparation method and application thereof

    CN105771954A

  • Rapid screening device and screening method for small-particle-size ternary materials

    CN118437052A