Titanium alloy surface modification method for imitating cementum ultrastructure and application of titanium alloy surface modification method

By constructing a dental cementum-like ultrastructure on the surface of titanium alloy, the problem of insufficient soft tissue sealing in titanium alloy surface modification technology is solved, cell adhesion and collagen fiber embedding are improved, and the long-term stability of implants is enhanced.

CN120844171APending Publication Date: 2025-10-28THE FIFTH AFFILIATED HOSPITAL SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510991916.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-18
Publication Date
2025-10-28

AI Technical Summary

Technical Problem

Existing titanium alloy surface modification technology has failed to effectively simulate the ultrastructure of cementum, resulting in insufficient soft tissue sealing at the implant neck, which easily leads to inflammation and affects the long-term stability of the implant.

Method used

After pickling with a mixture of nitric acid and hydrofluoric acid, a dental-like cementum ultrastructure is constructed on the surface of the titanium alloy by electrochemical anodizing, forming nanotubes or nanopores. Combined with mechanical polishing, a dental-like cementum microporous structure is prepared to promote collagen fiber anchoring and cell adhesion.

Benefits of technology

It significantly improves the hydrophilicity and cell adhesion of the titanium alloy surface, promotes the embedding and anchoring of collagen fibers, enhances soft tissue sealing, and improves the long-term stability of implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120844171A_ABST
    Figure CN120844171A_ABST
Patent Text Reader

Abstract

The invention discloses a cementum-imitating ultrastructure titanium alloy surface modification method and application thereof, and belongs to the technical field of biomedical material surface modification.The cementum-imitating ultrastructure titanium alloy surface modification method comprises the steps that S1, pretreatment is conducted, specifically, a titanium base material is subjected to ultrasonic cleaning with distilled water and absolute ethyl alcohol in sequence; immersing into mixed acid of nitric acid and hydrofluoric acid, and shaking and pickling for 1-3 minutes; s2, anodic oxidation: taking a titanium sheet as an anode and an inert electrode as a cathode; the electrolyte is an ethylene glycol aqueous solution containing 0.1-0.5 wt% of ammonium fluoride; applying direct-current constant voltage, and performing anodic oxidation; and S3, post-treatment: cleaning with acetone, absolute ethyl alcohol and distilled water in sequence, and carrying out vacuum drying. The titanium surface ultrastructure constructed by the method is similar to a cementum microstructure; an approach and an anchoring point are provided for attachment and penetration of surrounding soft tissue collagenous fibers; and popularization, application and industrial production are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomedical material surface modification technology, specifically relating to a method for modifying the surface of titanium alloys with a dental cementum-like ultrastructure and its application. Background Art

[0002] Titanium and its alloys have become the main material choice for dental implants due to their excellent corrosion resistance, good mechanical properties (such as high hardness, ultimate tensile strength and fatigue strength) and low elastic modulus, which can meet the basic requirements of human implants.

[0003] Titanium and its alloys come into direct contact with the gingival soft tissue in the perforation area. Their surface quality and morphology are crucial for maintaining gingival health and achieving good sealing of the peri-implant soft tissue, which directly affects the long-term stability and long-term outcome of the implant. Therefore, surface optimization treatment of implant components (especially abutments) made of pure titanium and its alloys to improve their integration with soft tissue is of significant necessity.

[0004] Currently, surface modification technologies for titanium materials mainly include mechanical methods (such as grinding, polishing, and sandblasting), physical methods (such as thermal spraying, vapor deposition, and ion implantation and deposition), and chemical methods (such as etching, anodizing, and chemical vapor deposition). These methods can improve the biocompatibility, biological activity, osteoconductivity, and corrosion resistance of titanium and its alloys to varying degrees. Among the many surface modification technologies, surface treatment based on electrochemical anodizing has significant advantages. This method can not only enhance the overall properties of titanium material surfaces but also construct specific nanoscale porous or tubular morphological structures on the material surface.

[0005] In the field of dental implantology, research and practice have shown that the nanopores or nanotubes created on the surface of titanium implants through anodizing can effectively promote the adhesion, proliferation, and differentiation of osteoblasts, thereby accelerating and enhancing the speed and quality of osseointegration. This micro-nano porous structure facilitates cell ingrowth into the pores, forming mechanical interlocking and enhancing cell adhesion and tissue integration. However, insufficient soft tissue sealing in the implant perforation area remains a persistent challenge. Poor sealing can easily lead to peri-implantitis, thereby disrupting established osseointegration and seriously threatening the long-term lifespan of the implant.

[0006] Theoretically, constructing specific porous structures (e.g., mimicking the ultrastructure of natural cementum) on the implant neck or abutment surface could create favorable conditions for the embedding and anchoring of connective tissue collagen fibers, thereby mimicking the physiological state of collagen fibers bound to cementum in natural periodontal tissues and potentially significantly improving soft tissue sealing. However, currently, there are no sufficiently researched or effectively disclosed solutions in the existing technology for processing and modifying titanium alloy surfaces to mimic the ultrastructure of cementum. Existing surface modification technologies (including nanotubes / pores formed by anodizing) mainly focus on promoting osseointegration, and there is a significant technological gap in their targeted design and effectiveness in promoting soft tissue sealing, especially in mimicking the ultrastructure of cementum. Summary of the Invention

[0007] To address the aforementioned deficiencies in existing technologies, this invention provides a method for surface modification of titanium alloys with dental cementum-like ultrastructures and its application, thereby solving the problem of insufficient soft tissue closure at the implant neck.

[0008] This invention is achieved through the following technical solution:

[0009] A method for surface modification of titanium alloys with a dental cementum-like ultrastructure, specifically including the following steps:

[0010] S1. Preprocessing:

[0011] The titanium substrate was ultrasonically cleaned sequentially with distilled water and anhydrous ethanol.

[0012] Immerse in a mixture of nitric acid and hydrofluoric acid and agitate for 1-3 minutes.

[0013] S2, Anodizing:

[0014] A titanium sheet is used as the anode, and an inert electrode is used as the cathode;

[0015] The electrolyte is an aqueous solution of ethylene glycol containing 0.1-0.5 wt% ammonium fluoride;

[0016] Anodizing is performed by applying a constant DC voltage.

[0017] S3, Post-processing:

[0018] Washed sequentially with acetone, anhydrous ethanol, and distilled water, and then vacuum dried.

[0019] Further, in step S1, the concentration of nitric acid is 0.1-0.5M and the concentration of hydrofluoric acid is 0.1-1.0M.

[0020] Furthermore, step S1 also includes a mechanical polishing step, wherein the mechanical polishing is performed by grinding the surface of the titanium substrate at a speed of 1000-9000 rpm, followed by cleaning with acetone, anhydrous ethanol, and distilled water in sequence and then drying.

[0021] Furthermore, in step S2, the volume concentration of the ethylene glycol aqueous solution is 10-90%.

[0022] Furthermore, in step S3, the DC constant voltage is 20-70V, and the reaction lasts from 2 minutes to 4 hours.

[0023] Secondly, the present invention also provides an application of a titanium alloy surface modification method for imitating dental cementum ultrastructure in the preparation of dental implants, wherein the titanium substrate surface has a microporous structure to promote gingival fibroblast anchoring and collagen fiber embedding.

[0024] Thirdly, the present invention also provides an oral implant abutment, the surface of which is modified by the above method to form a dentin-like cementum ultrastructure layer.

[0025] Compared with the prior art, the advantages of the present invention are as follows:

[0026] The present invention discloses a method for modifying the surface of titanium alloys to mimic the microstructure of dental cementum. The constructed titanium surface microstructure approximates the microstructure of dental cementum; it provides an entry point and anchoring point for the attachment and penetration of collagen fibers in surrounding soft tissue; and it is convenient for promotion, application and industrial production. Attached Figure Description

[0027] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn to scale.

[0028] Figure 1 This is the microstructure (SEM) of cementum after the removal of collagen fibers and other proteins; B represents the final details of A.

[0029] Figure 2 These are SEM images of titanium surface morphology structures prepared under different voltages and energizing durations. A and E show the control group samples with flat surfaces and no nanotubes under SEM. B and C show the experimental groups (30V and 40V) with titanium nanotubes of different diameters, exhibiting uniform diameter and a dense, orderly arrangement. D shows the 50V group with titanium nanotubes of varying sizes and disordered arrangement. F and G are 45° side views of the material surface, showing columnar titanium nanotubes in the 30V and 40V groups, and a conical shape in the 50V group (Example 1). Figure 1 Comparison of cementum ultrastructure shows that the ultrastructure of titanium surface is similar to that of cementum.

[0030] Figure 3The results show the hydrophilicity of titanium surfaces after different modification processes. Compared with the control group (A), the preparation of titanium nanotubes in groups B, C, and D significantly reduced the water contact angle of the material surface (Example 2). The comparison results show that the preparation of titanium nanotubes significantly improves the hydrophilicity of the material surface, which is beneficial to cell adhesion.

[0031] Figure 4 The images show the growth of fibroblasts on titanium surfaces treated with different modification processes (SEM). After one day of cell culture, the cells in the 30V and 40V groups completely transformed into a spindle-shaped morphology (B, C), with numerous protrusions extending from the cell surface into the nanotubes on the material surface (F, G). Conversely, the fibroblasts in the control group (A, E) and the 50V group (D, H) lacked obvious cell protrusions (Example 3). In vitro cell adhesion experiments further demonstrate that the preparation of titanium nanotubes significantly improved the hydrophilicity of the material surface, which is beneficial for cell adhesion. Detailed Implementation

[0032] To clearly and completely describe the technical solution and its specific working process of the present invention, the specific embodiments of the present invention are as follows, in conjunction with the accompanying drawings:

[0033] Example 1

[0034] This embodiment provides a method for surface modification of titanium alloys with simulated dental cement microstructures, specifically including the following steps:

[0035] (1) Clean the commercial pure titanium sheet (Guangzhou Anyou New Materials) with distilled water and anhydrous ethanol for 10 min each.

[0036] (2) Immerse the titanium sheet in a mixture of 0.254M HNO3 and 0.54M HF and agitate for 2 minutes. During this process, a large number of bubbles are generated in the solution, accompanied by exothermic reaction. After the process, rinse the titanium sheet with distilled water.

[0037] Then, a slow-speed turbine handpiece was used to polish the titanium sheet at 9000 rpm, followed by cleaning with acetone / ethanol / water for 5 minutes each, and then drying.

[0038] (3) In a 70% (w / v) ethylene glycol solution containing 0.25% (w / v) NH4F, titanium was used as the anode and copper rod as the cathode, and the reaction was carried out at a constant voltage of 30V for 2 minutes.

[0039] (4) After preparation, wash with acetone / ethanol / water for 5 minutes in sequence, and then vacuum dry.

[0040] Example 2

[0041] This embodiment provides a method for surface modification of titanium alloys with simulated dental cement microstructures, specifically including the following steps:

[0042] (1) Clean the titanium sheet with distilled water and anhydrous ethanol;

[0043] (2) Immerse the titanium sheet in a mixed acid solution of 0.254M nitric acid (HNO3) and 0.54M hydrofluoric acid (HF) for 2 minutes, shaking and acid washing. During this process, a large number of bubbles are generated in the solution, accompanied by exothermic reactions. After the acid washing is complete, rinse the titanium sheet with distilled water. Then, use a slow-speed turbine handpiece to polish the titanium sheet at a speed of 9000 rpm. Clean the sheet once each with acetone, anhydrous ethanol, and distilled water, for 5 minutes each time. Dry the titanium sheet for later use.

[0044] (3) Using a titanium sheet as the anode and a copper rod as the cathode, the electrodes were placed in a 70% (v / v) ethylene glycol solution containing 0.25% (w / v) ammonium fluoride and subjected to a constant DC voltage of 40V for 2 hours. After preparation, the electrodes were cleaned sequentially with acetone, anhydrous ethanol, and distilled water for 5 minutes each time.

[0045] (4) Add 1 drop of 10 μl distilled water to the surface of the titanium alloy specimen. After the droplet stabilizes, take a picture and calculate the water contact angle using the software in the instrument.

[0046] Example 3

[0047] This embodiment provides a method for surface modification of titanium alloys with simulated dental cement microstructures, specifically including the following steps:

[0048] (1) Clean the titanium sheet with distilled water and anhydrous ethanol;

[0049] (2) Immerse the titanium sheet in a mixed acid solution of 0.254M nitric acid (HNO3) and 0.54M hydrofluoric acid (HF) for 2 minutes, during which a large number of bubbles are generated in the solution and heat is released. After the process, rinse the titanium sheet with distilled water. Then, use a slow-speed turbine handpiece to polish the titanium sheet at a speed of 9000 rpm. Clean it once each with acetone, anhydrous ethanol, and distilled water, for 5 minutes each time. Dry the titanium sheet for later use.

[0050] (3) Using a titanium sheet as the anode and a copper rod as the cathode, the electrodes were placed in a 70% (v / v) ethylene glycol solution containing 0.25% (w / v) ammonium fluoride and subjected to a constant DC voltage of 40V for 2 hours. After preparation, the electrodes were cleaned sequentially with acetone, anhydrous ethanol, and distilled water for 5 minutes each time.

[0051] (4) Gingival fibroblasts were seeded onto titanium sheets (5×103 cells / well) and cultured at 37°C and 5% CO2 for 6 hours, 12 hours, 1 day and 4 days.

[0052] (5) At the end of the culture, discard the original culture medium and wash three times with PBS.

[0053] (6) Fix cells with 4% paraformaldehyde at room temperature for 30 minutes, then wash with PBS 3 times for 5 minutes each time.

[0054] (7) Prepare the sample and place it in a vacuum dryer at 37°C overnight.

[0055] (8) Use conductive adhesive to attach the sample to the test stage and spray gold for 20 seconds.

[0056] (9) After blowing off the surface gold powder, observe the sample under a scanning electron microscope.

[0057] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0058] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0059] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A method for surface modification of titanium alloys with a dental cementum-like ultrastructure, characterized in that, Specifically, the steps include the following: S1. Preprocessing: The titanium substrate was ultrasonically cleaned sequentially with distilled water and anhydrous ethanol. Immerse in a mixture of nitric acid and hydrofluoric acid and agitate for 1-3 minutes. S2, Anodizing: A titanium sheet is used as the anode, and an inert electrode is used as the cathode; The electrolyte is an aqueous solution of ethylene glycol containing 0.1-0.5 wt% ammonium fluoride; Anodizing is performed by applying a constant DC voltage. S3, Post-processing: Washed sequentially with acetone, anhydrous ethanol, and distilled water, and then vacuum dried.

2. The method for surface modification of titanium alloys with a dental cementum-like ultrastructure as described in claim 1, characterized in that, In step S1, the concentration of nitric acid is 0.1-0.5M and the concentration of hydrofluoric acid is 0.1-1.0M.

3. The method for surface modification of titanium alloys with a dental cementum-like ultrastructure as described in claim 1, characterized in that, Step S1 also includes a mechanical polishing step, wherein the surface of the titanium substrate is polished at a speed of 1000-9000 rpm, and then cleaned and dried in sequence with acetone, anhydrous ethanol, and distilled water.

4. The method for surface modification of titanium alloys with a dental cementum-like ultrastructure as described in claim 1, characterized in that, In step S2, the volume concentration of the ethylene glycol aqueous solution is 10-90%.

5. The method for surface modification of titanium alloys with a dental cementum-like ultrastructure as described in claim 1, characterized in that, In step S3, the DC constant voltage is 20-70V, and the reaction lasts from 2 minutes to 4 hours.

6. The application of the titanium alloy surface modification method for the dental cementum ultrastructure as described in claim 1 in the preparation of dental implants, characterized in that, The titanium substrate has a microporous structure on its surface, which promotes the anchoring of gingival fibroblasts and the embedding of collagen fibers.

7. A dental implant abutment, characterized in that, The surface of the abutment transgingival region is modified using the method described in any one of claims 1-5 to form a dentin-like cementum ultrastructure layer.