Anhydrous iron phosphate, a preparation method thereof, a positive electrode material, a positive electrode sheet, and a secondary battery

The preparation of rod-shaped anhydrous iron phosphate by hydrothermal method solves the problems of wide particle size distribution and large secondary particles in anhydrous iron phosphate, and improves the electrochemical performance of lithium iron phosphate cathode material, especially charge specific capacity, discharge specific capacity, rate performance and cycle life.

CN120841465BActive Publication Date: 2026-11-10HUBEI HONGRUN HIGH-TECH NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202511045606.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-28
Publication Date
2026-11-10
Estimated Expiration
2045-07-28

Smart Images

  • Figure CN120841465B_ABST
    Figure CN120841465B_ABST
Patent Text Reader

Abstract

The application provides anhydrous iron phosphate, a preparation method thereof, a positive electrode material, a positive electrode sheet and a secondary battery, and belongs to the technical field of secondary batteries, wherein the primary particles of the anhydrous iron phosphate are rod-shaped structures, and the ratio of the long axis length to the short axis length of the rod-shaped structure of the primary particles is (5.5-11.4):1. The primary particles of the anhydrous iron phosphate provided by the application are rod-shaped structures, and the ratio of the long axis length to the short axis length of the rod-shaped structure is (5.5-11.4):1, which is helpful to obtain anhydrous iron phosphate with concentrated primary particle size distribution, small secondary particles and sufficient active sites, so that the electrochemical performance of the positive electrode material prepared from the anhydrous iron phosphate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of secondary battery technology, and particularly relates to anhydrous iron phosphate and its preparation method, positive electrode material, positive electrode sheet and secondary battery. Background Technology

[0002] Lithium iron phosphate (LFP) batteries occupy an important position in the electric vehicle market due to their advantages such as safety, economy, and long cycle life, for example, in the application of batteries in the field of new energy vehicles. Iron phosphate is a key precursor for the preparation of lithium iron phosphate cathode materials, and its composition, iron-phosphorus ratio, morphology, crystal form, and other properties have a great influence on the physicochemical properties and electrochemical performance of lithium iron phosphate cathode materials.

[0003] Currently, the mainstream methods for preparing iron phosphate include: ① oxidation method and ② hydrothermal method. The oxidation method uses ferrous sulfate as the iron source, phosphoric acid or phosphate as the phosphorus source, and hydrogen peroxide as the oxidant. The pH of the reaction system is adjusted by adding ammonium salts or alkalis. After co-precipitation, aging, washing, and calcination, anhydrous iron phosphate meeting battery-grade standards is prepared. However, the oxidation method often requires the use of ammonium salts or alkalis to adjust the pH, resulting in the generation of large amounts of nitrates, sulfates, and ferric hydroxide impurities, leading to low product purity. The hydrothermal method involves a hydrothermal reaction of iron oxide, phosphoric acid, and reaction aids under high temperature and pressure, followed by washing and calcination to prepare anhydrous iron phosphate meeting battery-grade standards. However, the anhydrous iron phosphate prepared by the existing hydrothermal method has a wide particle size distribution and large secondary particles, resulting in non-uniformity in lithium iron phosphate cathode materials made from it during discharge. This means that the electrochemical performance of lithium iron phosphate cathode materials, such as discharge capacity, coulombic efficiency, and cycle life, needs improvement when applied to secondary batteries.

[0004] Therefore, it is necessary to propose a new anhydrous iron phosphate and its preparation method, cathode material, cathode sheet and secondary battery to solve the technical problem that the wide particle size distribution of anhydrous iron phosphate and the large size of secondary particles are not conducive to improving the electrochemical performance of lithium iron phosphate cathode materials prepared by anhydrous iron phosphate. Summary of the Invention

[0005] In view of the technical problems existing in the background art, this application provides anhydrous iron phosphate and its preparation method, cathode material, cathode sheet and secondary battery, aiming to solve the technical problem that the wide particle size distribution of anhydrous iron phosphate and the large secondary particles are not conducive to improving the electrochemical performance of lithium iron phosphate cathode material prepared by anhydrous iron phosphate.

[0006] In a first aspect, embodiments of this application provide anhydrous ferric phosphate, wherein the primary particles of the anhydrous ferric phosphate have a rod-like structure, and the ratio of the length of the major axis to the length of the minor axis of the rod-like structure of the primary particles is (5.5~11.4):1.

[0007] In the technical solution of this application embodiment, anhydrous iron phosphate is used as a precursor for preparing lithium iron phosphate. The morphology and size of its primary particles directly affect the performance of the lithium iron phosphate product. The primary particles are rod-shaped anhydrous iron phosphate, and the ratio of the long axis length to the short axis length of the rod-shaped structure of the primary particles meets the above-mentioned range. This helps to obtain anhydrous iron phosphate with a concentrated primary particle size distribution and small secondary particles, while having sufficient active sites, thereby improving the electrochemical performance of the cathode material prepared by anhydrous iron phosphate.

[0008] In some embodiments, the long axis length of the rod-shaped structure of the primary particle is 4170 nm to 5200 nm, and the short axis length of the rod-shaped structure of the primary particle is 455 nm to 755 nm.

[0009] In this embodiment, when the long axis length and short axis length of the rod-shaped structure of the primary particles of anhydrous iron phosphate meet the above-mentioned range, the long axis length distribution of the rod-shaped structure of the primary particles is concentrated, and the short axis length distribution of the rod-shaped structure of the primary particles is concentrated. This is beneficial to obtaining anhydrous iron phosphate with a concentrated particle size distribution of the secondary particles and a suitable ratio of long axis length to short axis length. This is beneficial to improving the electrochemical stability of the cathode material prepared by anhydrous iron phosphate while also taking into account the structural stability of the cathode material.

[0010] In some embodiments, the secondary particles of anhydrous ferric phosphate have a spherical morphology. The D50 particle size of the secondary particles of anhydrous ferric phosphate is 3 μm to 6.5 μm.

[0011] In this embodiment, the secondary particles have a near-spherical morphology and are more densely packed, which helps to increase the tap density of the material and thus improve the energy density of the cathode material prepared by anhydrous iron phosphate. When the particle size of the secondary particles of anhydrous iron phosphate meets the above-mentioned range, the particle size of the secondary particles of anhydrous iron phosphate is small and the distribution is concentrated, which helps to shorten the lithium ion solid-phase diffusion path in the cathode material prepared by anhydrous iron phosphate, thereby improving the rate performance, cycle performance and other electrochemical performance of the cathode material.

[0012] In some embodiments, the tap density of anhydrous ferric phosphate is 0.6 g / cm³. 3 ~1.2g / cm 3 The BET specific surface area of ​​anhydrous ferric phosphate is 4 m². 2 / g~12m 2 / g. The molar ratio of Fe to P in anhydrous ferric phosphate is 0.955~0.99. Anhydrous ferric phosphate has a monoclinic crystal form.

[0013] In this embodiment, when the tap density of anhydrous iron phosphate meets the above-mentioned range, the particles exhibit good compactness, which is beneficial for improving the charge specific capacity, discharge specific capacity, rate performance, energy density, and cycle life of the cathode material prepared from anhydrous iron phosphate. When the BET specific surface area of ​​anhydrous iron phosphate meets the above-mentioned range, it provides sufficient active sites, thereby further improving the electrochemical performance, such as cycle performance, of the cathode material prepared from anhydrous iron phosphate. When the molar ratio of Fe to P elements in anhydrous iron phosphate meets the above-mentioned range, the purity and stability of anhydrous iron phosphate are both high, which is beneficial for improving the overall performance of the cathode material prepared from anhydrous iron phosphate. When the crystal form of anhydrous iron phosphate is monoclinic, it promotes ion conduction, improves charging and discharging efficiency, and extends the service life of the cathode material prepared from anhydrous iron phosphate, thereby improving the electrochemical performance and performance stability of the cathode material prepared from anhydrous iron phosphate.

[0014] Secondly, embodiments of this application provide a method for preparing anhydrous ferric phosphate, comprising the following steps: Iron oxide and phosphoric acid solution were mixed and subjected to a first reaction treatment to obtain a first mixture; The first mixture, ferrous salt and oxidant are mixed and subjected to a second reaction treatment to obtain ferric phosphate dihydrate slurry; Anhydrous ferric phosphate was obtained by solid-liquid separation and sintering of dihydrate ferric phosphate slurry.

[0015] Among them, the primary particles of anhydrous ferric phosphate have a rod-like structure, and the ratio of the length of the major axis to the length of the minor axis of the rod-like structure of the primary particles is (5.5~11.4):1.

[0016] In the technical solution of this application embodiment, iron oxide and phosphoric acid solution are first mixed and subjected to a first reaction treatment to obtain a first mixture containing crystalline monoclinic ferric phosphate dihydrate; the first mixture, ferrous salt, and oxidant are mixed and subjected to a second reaction treatment, using the ferric phosphate dihydrate obtained from the first reaction treatment as seed crystals, and further subjected to a second reaction treatment to obtain ferric phosphate dihydrate slurry; the ferric phosphate dihydrate slurry is subjected to solid-liquid separation treatment and sintering treatment to obtain anhydrous ferric phosphate. Compared with other preparation methods such as solid-phase synthesis method, homogeneous precipitation method, and oxidation method, the preparation method provided in this application obtains crystalline monoclinic ferric phosphate dihydrate through a hydrothermal method, then uses the monoclinic ferric phosphate dihydrate obtained by the hydrothermal method as seed crystals to obtain ferric phosphate dihydrate through a co-precipitation method, and finally uses the ferric phosphate dihydrate for sintering treatment to obtain anhydrous ferric phosphate. The ferric phosphate dihydrate has complete crystal grains, a low degree of particle agglomeration, and the raw materials are cheap and readily available. The obtained anhydrous ferric phosphate has complete crystal grains, and the secondary particles have small particle size and concentrated distribution. The anhydrous iron phosphate obtained by the preparation method provided in this application has a rod-shaped primary particle structure, and the ratio of the long axis length to the short axis length of the rod-shaped primary particle meets the above-mentioned range. This helps to obtain anhydrous iron phosphate with a concentrated primary particle size distribution and small secondary particles, while having sufficient active sites, thereby improving the electrochemical performance of the cathode material prepared by anhydrous iron phosphate.

[0017] In some embodiments, the molar ratio of iron oxide to phosphoric acid in the phosphoric acid solution is 1:(8~15). The mass fraction of phosphoric acid in the phosphoric acid solution is 30%~40%. The temperature of the first reaction treatment is 100℃~200℃, the pressure of the first reaction treatment is 0.3MPa~0.8MPa, and the time of the first reaction treatment is 1h~2.5h.

[0018] In this embodiment, when the molar ratio of iron oxide to phosphoric acid in the phosphoric acid solution meets the above conditions, phosphoric acid is significantly in excess, which helps to completely react the iron oxide and facilitates the preparation of crystalline ferric phosphate dihydrate under high temperature and high pressure conditions. When the temperature, time, and pressure of the first reaction treatment meet the above ranges, it helps to complete the reaction and obtain a sufficient amount of crystalline ferric phosphate dihydrate, so as to provide a suitable number of seed crystals for the second reaction treatment and facilitate the control of the morphology of the finally obtained anhydrous ferric phosphate, so that the anhydrous ferric phosphate has a rod-like structure and the ratio of the long axis length to the short axis length of the rod-like structure is (5.5~11.4):1.

[0019] In some embodiments, the ferrous salt is at least one of ferrous sulfate, ferrous chloride, or ferrous nitrate. The oxidant is at least one of hydrogen peroxide, sodium peroxide, potassium peroxide, sodium hypochlorite, potassium hypochlorite, sodium persulfate, potassium persulfate, or ozone. The molar ratio of ferrous salt to ferric oxide is (4~9):1. The molar ratio of ferrous salt to oxidant is 1:(0.5~0.8).

[0020] In this embodiment, when the molar ratio of ferrous salt to ferric oxide meets the above-mentioned range, it is beneficial to control the growth degree of ferric phosphate dihydrate crystals in the second reaction treatment, thereby obtaining anhydrous ferric phosphate with a suitable ratio of the long axis length to the short axis length of the primary particles and a concentrated particle size in the secondary particles. When the molar ratio of ferrous salt to oxidant meets the above-mentioned range, it allows Fe... 2+ It allows for a more complete reaction with the oxidant and avoids wasting the oxidant.

[0021] In some embodiments, the step of mixing the first mixture, the ferrous salt, and the oxidant for a second reaction treatment to obtain ferric phosphate dihydrate slurry includes: Ferrous salt and oxidant are mixed to form a first mixture at a first mixing temperature and for a first mixing time to obtain a second mixture; The second mixture, after undergoing a second reaction at a second reaction temperature and a second reaction time, yields ferric phosphate dihydrate slurry; in, The first mixing temperature is 20℃~30℃, and the first mixing time is 10min~30min; The second reaction temperature is 90℃~98℃, the second reaction time is 30min~80min, and the second reaction is carried out under stirring conditions.

[0022] In this embodiment, a second mixture is obtained by mixing ferrous salt and oxidant to a first mixture at a first mixing temperature and for a first mixing time; the second mixture is then subjected to a second reaction temperature and a second reaction time to allow amorphous ferric phosphate to undergo sufficient crystal transformation to form ferric phosphate dihydrate, thereby obtaining ferric phosphate dihydrate slurry.

[0023] In some embodiments, the sintering temperature is 550°C to 700°C, the sintering time is 2 hours to 4 hours, and the sintering atmosphere is air.

[0024] In this embodiment, when the sintering temperature and time meet the above range, ferric phosphate dihydrate is fully converted through high-temperature calcination to form high-purity anhydrous ferric phosphate with a suitable ratio of the long axis length to the short axis length of the primary particles and a concentrated particle size of the secondary particles.

[0025] Thirdly, embodiments of this application provide a positive electrode material, which is lithium iron phosphate or lithium manganese iron phosphate prepared by using the above-mentioned anhydrous iron phosphate or anhydrous iron phosphate prepared by the above-mentioned method of anhydrous iron phosphate as a precursor.

[0026] In the technical solution of this application embodiment, the positive electrode material is prepared by using the above-mentioned anhydrous iron phosphate as a precursor, and thus has good charge specific capacity, discharge specific capacity, rate performance, energy density and cycle life.

[0027] Fourthly, embodiments of this application provide a positive electrode sheet, which includes the aforementioned positive electrode material.

[0028] In the technical solution of this application embodiment, the positive electrode sheet contains the above-mentioned positive electrode material, and thus has good charge specific capacity, discharge specific capacity, rate performance, energy density and cycle life.

[0029] Fifthly, embodiments of this application provide a secondary battery, which includes the aforementioned positive electrode plate.

[0030] In the technical solution of this application embodiment, the secondary battery includes the above-mentioned positive electrode sheet, and thus has good charging specific capacity, discharging specific capacity, rate performance, energy density and cycle life.

[0031] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0032] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0033] Figure 1 These are XRD results of anhydrous ferric phosphate provided in Examples 1-4 of this application; Figure 2 This is the first SEM result image of anhydrous ferric phosphate provided in Example 1 of this application; Figure 3 This is a second SEM result image of anhydrous ferric phosphate provided in Example 1 of this application; Figure 4 This is the first SEM result image of anhydrous ferric phosphate provided in Example 2 of this application; Figure 5 This is a second SEM result image of anhydrous ferric phosphate provided in Example 2 of this application; Figure 6 This is the first SEM result image of anhydrous ferric phosphate provided in Example 3 of this application; Figure 7 This is a second SEM result image of anhydrous ferric phosphate provided in Example 3 of this application; Figure 8 This is the first SEM result image of anhydrous iron phosphate provided in Comparative Example 1 of this application; Figure 9This is a second SEM image of anhydrous ferric phosphate provided in Comparative Example 1 of this application. Detailed Implementation

[0034] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0036] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0037] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0038] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0039] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0040] In the description of the embodiments of this application, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0041] In the description of the embodiments of this application, "ppm" means the mass of the tested element, molecule or ion in parts per million of the sample mass.

[0042] In the description of the embodiments of this application, unless otherwise specified, the solvent in "solution" and "washing liquid" is selected from at least one of distilled water, deionized water, deionized water, pure water, and ultrapure water.

[0043] In existing technologies, when preparing iron phosphate via hydrothermal methods, the resulting anhydrous iron phosphate exhibits poor crystallinity and a wide particle size distribution. Small particles act as a co-solvent, causing large particles to agglomerate. This results in large secondary particles with low BET, leading to non-uniformity in lithium iron phosphate cathode materials prepared using it as a precursor during discharge. Consequently, the electrochemical performance of lithium iron phosphate cathode materials, such as discharge capacity, coulombic efficiency, and cycle life, needs improvement when applied to secondary batteries.

[0044] To address the problem that existing hydrothermal methods produce anhydrous iron phosphate with a wide particle size distribution and large secondary particles, which is detrimental to improving the electrochemical performance of lithium iron phosphate cathode materials prepared from anhydrous iron phosphate, this application provides anhydrous iron phosphate, its preparation method, cathode material, cathode sheet, and secondary battery.

[0045] In one aspect, embodiments of this application provide anhydrous ferric phosphate, wherein the primary particles of the anhydrous ferric phosphate have a rod-like structure, and the ratio of the length of the major axis to the length of the minor axis of the rod-like structure of the primary particles is (5.5~11.4):1, including but not limited to 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.2:1, 11.4:1, etc.

[0046] Specifically, battery-grade anhydrous iron phosphate comprises several secondary particles, which are composed of several primary particles. It should be noted in this application that, since each rod-shaped structure has a different length, the ratio of the major axis length to the minor axis length of the rod-shaped structure of the primary particles mentioned in this application is the ratio of the major axis length of each rod-shaped structure to the minor axis length of that rod-shaped structure.

[0047] In the technical solution of this application embodiment, anhydrous iron phosphate is used as a precursor for preparing lithium iron phosphate. The morphology and size of its primary particles directly affect the performance of the lithium iron phosphate product. The primary particles are rod-shaped anhydrous iron phosphate, and the ratio of the long axis length to the short axis length of the rod-shaped structure of the primary particles meets the above-mentioned range. This helps to obtain anhydrous iron phosphate with a concentrated primary particle size distribution and small secondary particles, while having sufficient active sites, thereby improving the electrochemical performance of the cathode material prepared by anhydrous iron phosphate.

[0048] Furthermore, in some embodiments, the ratio of the long axis length to the short axis length of the rod-shaped structure of the primary particles is (6.8~10.7):1. Controlling the ratio of the long axis length to the short axis length within this range helps to further optimize the morphology of anhydrous iron phosphate and improve the electrochemical performance of the cathode material prepared by anhydrous iron phosphate.

[0049] Furthermore, in some embodiments, the long axis length of the rod-shaped structure of the primary particle is 4170 nm to 5200 nm, including but not limited to 4170 nm, 4370 nm, 4570 nm, 4770 nm, 4970 nm, 5097 nm, 5199 nm, 5200 nm, etc., and the short axis length of the rod-shaped structure of the primary particle is 455 nm to 755 nm, including but not limited to 455 nm, 463 nm, 500 nm, 540 nm, 580 nm, 620 nm, 660 nm, 700 nm, 734 nm, 755 nm, etc.

[0050] In the technical solution of this application embodiment, when the long axis length and short axis length of the rod-shaped structure of the primary particles of anhydrous iron phosphate meet the above range, the long axis length distribution of the rod-shaped structure of the primary particles is concentrated, and the short axis length distribution of the rod-shaped structure of the primary particles is concentrated. This is beneficial to obtaining anhydrous iron phosphate with a concentrated particle size distribution of the secondary particles and a suitable ratio of long axis length to short axis length. This is beneficial to improving the electrochemical stability of the cathode material prepared by anhydrous iron phosphate while taking into account the structural stability of the cathode material.

[0051] Furthermore, in some embodiments, the long axis length of the rod-shaped structure of the primary particles is 4170 nm to 5076 nm, and the short axis length of the rod-shaped structure of the primary particles is 463 nm to 721 nm. This helps to obtain anhydrous iron phosphate with a more concentrated particle size distribution and a suitable ratio of long axis length to short axis length. This is beneficial to improving the electrochemical stability of the cathode material prepared by anhydrous iron phosphate while also taking into account the structural stability of the cathode material.

[0052] Furthermore, in some embodiments, the secondary particles of anhydrous ferric phosphate have a spherical morphology.

[0053] In the technical solution of this application embodiment, the secondary particles have a spherical morphology and are more tightly packed between particles, which is beneficial to improving the tap density of the material and thus improving the energy density of the cathode material prepared by anhydrous iron phosphate.

[0054] Furthermore, in some embodiments, the D50 particle size of the anhydrous ferric phosphate is 3μm to 6.5μm, including but not limited to 3μm, 4μm, 5μm, 6μm, 6.5μm, etc. Further, the D50 particle size of the anhydrous ferric phosphate is 4.0μm to 4.7μm.

[0055] In the technical solution of this application embodiment, when the particle size of anhydrous iron phosphate meets the above range, the particle size of anhydrous iron phosphate is small and the distribution is concentrated, which helps to shorten the lithium ion solid-phase diffusion path in the cathode material prepared by anhydrous iron phosphate, thereby improving the rate performance, cycle life and other electrochemical performance of the cathode material.

[0056] Furthermore, in some embodiments, the tap density of anhydrous ferric phosphate is 0.6 g / cm³. 3 ~1.2g / cm 3 Including but not limited to 0.6g / cm 3 0.8g / cm 3 1g / cm 3 1.2g / cm 3 Furthermore, the tap density of the anhydrous ferric phosphate is 0.7 g / cm³. 3 ~1.1g / cm 3 .

[0057] In the technical solution of this application embodiment, when the tap density of anhydrous iron phosphate meets the above range, the particles have a good degree of compactness, which is beneficial to improving the charging specific capacity, discharging specific capacity, rate performance, energy density and cycle life of the cathode material prepared by anhydrous iron phosphate.

[0058] Furthermore, in some embodiments, the BET specific surface area of ​​anhydrous ferric phosphate is 4 m². 2 / g~12m 2 / g, including but not limited to 4m 2 / g、6m 2 / g、8m 2 / g、9m 2 / g, 10m 2 / g、11m 2 / g、12m 2 / g, etc. Furthermore, the BET specific surface area of ​​the anhydrous ferric phosphate is 8m². 2 / g~10.5m 2 / g.

[0059] In the technical solution of this application embodiment, when the BET specific surface area of ​​anhydrous iron phosphate meets the above-mentioned range, it is beneficial to provide sufficient active sites, thereby further improving the electrochemical performance such as cycle performance of the cathode material prepared by anhydrous iron phosphate. If the specific surface area is too large, it will lead to too many gaps between particles, thereby hindering the improvement of compaction density; if the specific surface area is too small, it will lead to excessively large particle size, thereby affecting the insertion and extraction of lithium ions.

[0060] Furthermore, in some embodiments, the molar ratio of Fe to P in anhydrous ferric phosphate is 0.955~0.99, including but not limited to 0.965, 0.97, 0.975, 0.98, 0.985, 0.99, etc. Even further, the molar ratio of Fe to P in anhydrous ferric phosphate can be 0.965~0.99.

[0061] In the technical solution of this application embodiment, when the molar ratio of Fe to P in anhydrous iron phosphate meets the above range, the purity and stability of anhydrous iron phosphate are both high, which is beneficial to improving the overall performance of the cathode material prepared by anhydrous iron phosphate.

[0062] Furthermore, in some embodiments, the anhydrous iron phosphate has a monoclinic crystal form.

[0063] In the technical solution of this application embodiment, when the crystal form of anhydrous iron phosphate is monoclinic, it promotes the ion conduction of the cathode material prepared by anhydrous iron phosphate, improves the charging and discharging efficiency, and extends the service life, thereby improving the electrochemical performance and performance stability of the cathode material prepared by anhydrous iron phosphate.

[0064] Furthermore, in some embodiments, the anhydrous ferric phosphate has a low impurity content, and the content of each impurity can be controlled within the following ranges: 0ppm≤Al≤172.21ppm, 0ppm≤Ca≤10.9ppm, 0ppm≤Cd≤0.49ppm, 0ppm≤Co≤9.48ppm, 0ppm≤Cr≤8.31ppm, 0ppm≤Cu≤0.9ppm, 0ppm≤Mg≤138.26ppm, 0ppm≤Mn≤138.81ppm, 0ppm≤Ni≤37.56ppm, and 0ppm≤Pb≤36.97ppm. Furthermore, the impurity content of anhydrous ferric phosphate can even reach the following standards: 0ppm≤Al≤131.22ppm, 0ppm≤Ca≤7.32ppm, 0ppm≤Cd≤0.42ppm, 0ppm≤Co≤8.22ppm, 0ppm≤Cr≤6.6ppm, 0ppm≤Cu≤0.9ppm, 0ppm≤Mg≤105.86ppm, 0ppm≤Mn≤97.68ppm, 0ppm≤Ni≤27.96ppm, and 0ppm≤Pb≤17.35ppm.

[0065] Furthermore, in some embodiments, the cathode material prepared using the anhydrous iron phosphate proposed in the embodiments of this application exhibits high compaction density and electrochemical performance. For example, the compaction density can reach 2.3 g / cm³. 3 ~2.5g / cm 3 The initial charge specific capacity can reach 155mAh / g~166mAh / g, the initial discharge specific capacity can reach 149mAh / g~159mAh / g, and the initial coulombic efficiency can reach over 93.7%. Furthermore, the compaction density of the cathode material prepared using the anhydrous iron phosphate method proposed in this application reaches 2.4g / cm³. 3 ~2.5g / cm 3 The initial charge specific capacity reaches 158mAh / g~166mAh / g, the initial discharge specific capacity reaches 156mAh / g~159mAh / g, and the initial coulombic efficiency reaches 97.3%~99%.

[0066] Secondly, embodiments of this application provide a method for preparing anhydrous ferric phosphate, comprising the following steps: Iron oxide and phosphoric acid solution were mixed and subjected to a first reaction treatment to obtain a first mixture; The first mixture, ferrous salt and oxidant are mixed and subjected to a second reaction treatment to obtain ferric phosphate dihydrate slurry; Anhydrous ferric phosphate was obtained by solid-liquid separation and sintering of dihydrate ferric phosphate slurry.

[0067] Among them, the primary particles of anhydrous ferric phosphate have a rod-like structure, and the ratio of the length of the major axis to the length of the minor axis of the rod-like structure of the primary particles is (5.5~11.4):1, including but not limited to 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.2:1, 11.4:1, etc.

[0068] In the technical solution of this application embodiment, iron oxide and phosphoric acid solution are first mixed and subjected to a first reaction treatment to obtain a first mixture containing crystalline monoclinic ferric phosphate dihydrate; the first mixture, ferrous salt, and oxidant are mixed and subjected to a second reaction treatment, using the ferric phosphate dihydrate obtained from the first reaction treatment as seed crystals, and further subjected to a second reaction treatment to obtain ferric phosphate dihydrate slurry; the ferric phosphate dihydrate slurry is subjected to solid-liquid separation treatment and sintering treatment to obtain anhydrous ferric phosphate. Compared with other preparation methods such as solid-phase synthesis method, homogeneous precipitation method, and oxidation method, the preparation method provided in this application obtains crystalline monoclinic ferric phosphate dihydrate through a hydrothermal method, then uses the ferric phosphate dihydrate obtained by the hydrothermal method as seed crystals to obtain ferric phosphate dihydrate through a co-precipitation method, and finally uses the ferric phosphate dihydrate for sintering treatment to obtain anhydrous ferric phosphate. The ferric phosphate dihydrate has complete crystal grains, a low degree of particle agglomeration, and the raw materials are cheap and readily available. The obtained anhydrous ferric phosphate has complete crystal grains, and the secondary particles have small particle sizes and concentrated distribution. This application uses simple raw materials, requires no ammonia nitrogen, and reduces the need for other auxiliary materials, effectively lowering production costs, reducing wastewater and sewage generation, and protecting water resources. The method described in this application not only yields battery-grade iron phosphate but also enables the recycling of phosphoric acid. Furthermore, the process is simple, low-cost, and conducive to large-scale production. The anhydrous iron phosphate obtained by the preparation method provided in this application has rod-shaped primary particles, and the ratio of the long axis length to the short axis length of the rod-shaped primary particles meets the aforementioned range. This helps to obtain anhydrous iron phosphate with a concentrated primary particle size distribution and small secondary particles, while possessing sufficient active sites, thereby improving the electrochemical performance of the cathode material prepared from anhydrous iron phosphate.

[0069] The chemical reaction equations involved in the first reaction process are as follows: Fe₂O₃ + 2H₃PO₄ + H₂O = 2FePO₄·2H₂O In this application, it should be noted that the solid-liquid separation process includes solid-liquid separation, washing, and drying, which are existing technologies and will not be described in detail here. For example, washing is performed until the conductivity of the washing liquid is ≤350μs / cm; the drying temperature is 80℃~120℃, and the drying time is 5h~10h. In traditional oxidation methods, at least two solid-liquid separations and multiple rinsing steps are often required to control the conductivity of the washing liquid to below 350μs / cm to obtain a product that meets the requirements. However, in the preparation method provided in the embodiments of this application, the synthesis steps are optimized so that only one solid-liquid separation and rinsing step is required, simplifying the steps, improving production efficiency, and helping to reduce energy consumption and save resources.

[0070] Furthermore, in some embodiments, the molar ratio of iron oxide to phosphoric acid in the phosphoric acid solution is 1:(8~15).

[0071] In the technical solution of this application embodiment, when the molar ratio of iron oxide to phosphoric acid in the phosphoric acid solution meets the above conditions, phosphoric acid is significantly in excess, which helps to completely react the iron oxide and facilitates the preparation of crystalline ferric phosphate dihydrate under high temperature and high pressure conditions. If the amount of phosphoric acid added is too low, the iron oxide reaction will be incomplete; if the amount of phosphoric acid added is too high, it will not only lead to excessive phosphoric acid and high raw material costs, but also result in excessively high phosphoric acid concentration, increased solution viscosity, hindering the diffusion of iron ions and affecting the nucleation and crystallization of ferric phosphate. In addition, the higher the phosphoric acid concentration, the lower the pH value after the reaction, and the dynamic equilibrium of precipitation and dissolution of ferric phosphate leads to a decrease in the reaction rate.

[0072] Furthermore, in some embodiments, the iron oxide is iron oxide red.

[0073] Iron oxide red is widely available and cheaper than raw materials such as ferrous salts. In the technical solution of this application embodiment, by optimizing the process route, anhydrous ferric phosphate is prepared by first reacting iron oxide red with phosphoric acid solution and then adding ferrous salt. Compared with traditional oxidation methods, this reduces the proportion of ferrous salt in the raw materials, which is more conducive to controlling raw material costs.

[0074] Furthermore, in some embodiments, the mass fraction of phosphoric acid in the phosphoric acid solution is 30% to 40%, including but not limited to 30%, 32%, 34%, 36%, 38%, 40%, etc.

[0075] Furthermore, in some embodiments, the temperature of the first reaction treatment is 100℃~200℃, including but not limited to 100℃, 120℃, 150℃, 180℃, 200℃, etc.; the pressure of the first reaction treatment is 0.3MPa~0.8MPa, including but not limited to 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, 0.7MPa, 0.8MPa, etc.; and the time of the first reaction treatment is 1h~2.5h, including but not limited to 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, etc.

[0076] In the technical solution of this application embodiment, when the temperature, time, and pressure of the first reaction treatment meet the above-mentioned ranges, it helps to complete the reaction and obtain a sufficient amount of crystalline ferric phosphate dihydrate. This facilitates the provision of a suitable number of seed crystals for the second reaction treatment, and makes it easier to control the morphology of the finally obtained anhydrous ferric phosphate, so that the anhydrous ferric phosphate has a rod-like structure and the ratio of the long axis length to the short axis length of the rod-like structure is (5.5~11.4):1. If the temperature, time, and pressure of the first reaction treatment are too low, the reaction will be incomplete; if the temperature of the first reaction treatment is too high, the growth rate of ferric phosphate will be greater than the crystal transformation rate, resulting in larger secondary particles and a smaller BET specific surface area; if the time of the first reaction treatment is too long, it will cause energy waste and affect the production cycle.

[0077] Furthermore, in some embodiments, the ferrous salt is at least one of ferrous sulfate, ferrous chloride, or ferrous nitrate.

[0078] Furthermore, in some embodiments, the oxidant is at least one selected from hydrogen peroxide, sodium peroxide, potassium peroxide, sodium hypochlorite, potassium hypochlorite, sodium persulfate, potassium persulfate, and ozone.

[0079] Furthermore, in some embodiments, the oxidant is hydrogen peroxide, and the mass fraction of hydrogen peroxide is 25% to 30%, including but not limited to 25%, 26%, 27%, 28%, 29%, 30%, etc.

[0080] Furthermore, in some embodiments, the molar ratio of ferrous salt to ferric oxide is (4~9):1, including but not limited to 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, etc.

[0081] In the technical solution of this application embodiment, when the molar ratio of ferrous salt to ferric oxide meets the above-mentioned range, it is beneficial to control the growth degree of ferric phosphate dihydrate crystals in the second reaction treatment, thereby obtaining anhydrous ferric phosphate with a suitable ratio of the long axis length to the short axis length of the primary particles and a concentrated particle size of the secondary particles. If the proportion of ferrous salt is too low, it will result in the inability to completely consume the phosphorus in the mother liquor; if the proportion of ferrous salt is too high, it will result in difficulty in subsequent rinsing, increase the water consumption, and ultimately lead to excessive sulfur content in the anhydrous ferric phosphate product.

[0082] Furthermore, in some embodiments, the molar ratio of ferrous salt to oxidant is 1:(0.5~0.8), including but not limited to 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, etc.

[0083] In the technical solution of this application embodiment, when the molar ratio of ferrous salt to oxidant satisfies the above-mentioned range, Fe... 2+ This ensures a more complete reaction with the oxidant and avoids wasting the oxidant. If the amount of oxidant added is too low, it will result in incomplete Fe... 2+ Oxidized to Fe 3+ This can affect the purity, stability, and electrochemical performance of the material. If the amount of oxidant added is too high, it can easily trigger unnecessary side reactions, which will also adversely affect the purity and electrochemical performance of the material.

[0084] Further, in some embodiments, the step of mixing the first mixture, the ferrous salt, and the oxidant for a second reaction treatment to obtain ferric phosphate dihydrate slurry includes: Ferrous salt and oxidant are mixed to form a first mixture at a first mixing temperature and for a first mixing time to obtain a second mixture; The second mixture, after undergoing a second reaction at a second reaction temperature and a second reaction time, yields ferric phosphate dihydrate slurry; The first mixing temperature is 20℃~30℃, including but not limited to 20℃, 22℃, 24℃, 26℃, 28℃, 30℃, etc., and the first mixing time is 10min~30min.

[0085] The second reaction temperature is 90℃~98℃, including but not limited to 90℃, 92℃, 94℃, 96℃, 98℃, etc., and the second reaction time is 30min~80min, including but not limited to 30min, 40min, 50min, 60min, 70min, 80min, etc., and the second reaction is carried out under stirring conditions, with a stirring rate of 100~200r / min, including but not limited to 100r / min, 120r / min, 140r / min, 160r / min, 180r / min, 200r / min, etc.

[0086] In the technical solution of this application embodiment, a second mixture is obtained by mixing ferrous salt and oxidant at a first mixing temperature for a first mixing time; the second mixture is then subjected to a second reaction temperature for a second reaction time, allowing amorphous ferric phosphate to undergo sufficient crystal transformation to form ferric phosphate dihydrate, thus obtaining ferric phosphate dihydrate slurry. If the second reaction temperature is too low, the amorphous ferric phosphate will not be completely converted into ferric phosphate dihydrate, which will adversely affect the purity and performance of the final product; if the second reaction temperature is too high, the crystal growth rate will be accelerated, resulting in excessively large grain size, which will adversely affect the specific surface area and ion diffusion path of the material.

[0087] Specifically, ferrous salt and oxidant are mixed into a first mixture at a first mixing temperature and for a first mixing time by dropwise addition.

[0088] In the technical solution of this application embodiment, the dropwise addition method helps to avoid local overheating or violent reaction caused by rapid reaction, and ensures that the reaction proceeds smoothly.

[0089] Furthermore, in some embodiments, the sintering temperature is 550℃~700℃, including but not limited to 550℃, 600℃, 650℃, 700℃, etc., the sintering time is 2h~4h, including but not limited to 2h, 2.5h, 3h, 3.5h, 4h, etc., and the sintering atmosphere is air.

[0090] In the technical solution of this application embodiment, when the sintering temperature and time meet the above-mentioned range, ferric phosphate dihydrate can be fully converted through high-temperature calcination to form high-purity anhydrous ferric phosphate with a suitable ratio of the long axis length to the short axis length of the primary particles and a concentrated particle size of the secondary particles. If the sintering temperature is too low or the time is too short, the crystal growth momentum is insufficient, and anhydrous ferric phosphate with small particles and incomplete crystal form is easily formed, which manifests as rough crystal surface and uneven particle size distribution, thereby affecting the specific surface area and electrochemical performance of the cathode material formed from anhydrous ferric phosphate as raw material. If the sintering temperature is too high or the time is too long, it will promote excessive crystal growth, forming anhydrous ferric phosphate particles with excessively large particle size, or even agglomeration. The dispersion of the agglomerated particles becomes poor, and the prepared cathode material is difficult to disperse uniformly in the battery slurry preparation, affecting the electrode performance, requiring more energy consumption, and increasing production costs.

[0091] Thirdly, embodiments of this application provide a positive electrode material, which is lithium iron phosphate or lithium manganese iron phosphate prepared by using the above-mentioned anhydrous iron phosphate or anhydrous iron phosphate prepared by the above-mentioned method of anhydrous iron phosphate as a precursor.

[0092] In the technical solution of this application embodiment, the positive electrode material is prepared by using the above-mentioned anhydrous iron phosphate as a precursor, and thus has good charge specific capacity, discharge specific capacity, rate performance, energy density and cycle life.

[0093] Fourthly, embodiments of this application provide a positive electrode sheet, which includes the aforementioned positive electrode material.

[0094] In the technical solution of this application embodiment, the positive electrode sheet contains the above-mentioned positive electrode material, and thus has good charge specific capacity, discharge specific capacity, rate performance, energy density and cycle life.

[0095] Fifthly, embodiments of this application provide a secondary battery, which includes the aforementioned positive electrode plate.

[0096] In the technical solution of this application embodiment, the secondary battery includes the above-mentioned positive electrode sheet, and thus has good charging specific capacity, discharging specific capacity, rate performance, energy density and cycle life.

[0097] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0098] I. Preparation Method Example 1 (1) At room temperature, iron oxide red (0.75 mol) and phosphoric acid solution (the mass fraction of phosphoric acid is 33.3% and the molar amount of phosphoric acid is 9.75 mol) are mixed and stirred evenly, and then added to a high-pressure reactor. The reaction is carried out at 150℃ for 2 hours with a reaction pressure of 0.4 MPa. After the reaction is complete, the pressure is released to obtain the first mixture.

[0099] (2) Ferrous sulfate solution (21% ferrous sulfate by mass and 6.0 mol ferrous sulfate by molar amount) and hydrogen peroxide (27.5% hydrogen peroxide by mass and 3.6 mol hydrogen peroxide by molar amount) were added dropwise to the reactor at 25°C. The addition was completed in 20 min. Then, the mixture was stirred at 95°C for 75 min at a stirring rate of 150 r / min to obtain ferric phosphate dihydrate slurry.

[0100] (3) After solid-liquid separation, the ferric phosphate dihydrate slurry was rinsed until the conductivity of the washing liquid was ≤350μs / cm, then dried at 95℃ for 7h, and finally sintered at 600℃ for 3h to obtain anhydrous ferric phosphate.

[0101] Example 2 The difference between this embodiment and Example 1 is that the amount of iron oxide red added is adjusted to 1.25 mol, the amount of phosphoric acid added is adjusted to 16.25 mol, the amount of ferrous sulfate added is adjusted to 5.0 mol, and the amount of hydrogen peroxide added is adjusted to 3 mol.

[0102] Example 3 The difference between this embodiment and Example 1 is that the amount of iron oxide red added is adjusted to 0.69 mol, the amount of phosphoric acid added is adjusted to 8.97 mol, the amount of ferrous sulfate added is adjusted to 6.12 mol, and the amount of hydrogen peroxide added is adjusted to 3.672 mol.

[0103] Example 4 The difference between this embodiment and Example 1 is that the amount of iron oxide red added is adjusted to 0.65 mol, the amount of phosphoric acid added is adjusted to 8.45 mol, the amount of ferrous sulfate added is adjusted to 6.2 mol, and the amount of hydrogen peroxide added is adjusted to 3.72 mol.

[0104] Example 5 The difference between this embodiment and Example 1 is that the amount of iron oxide red added is adjusted to 1.3 mol, the amount of phosphoric acid added is adjusted to 16.9 mol, the amount of ferrous sulfate added is adjusted to 4.9 mol, and the amount of hydrogen peroxide added is adjusted to 2.94 mol.

[0105] Example 6 The difference between this embodiment and Embodiment 1 is that the amount of hydrogen peroxide added is adjusted to 3.3 mol.

[0106] Example 7 The difference between this embodiment and Embodiment 1 is that the amount of hydrogen peroxide added is adjusted to 4.5 mol.

[0107] Example 8 The difference between this embodiment and Embodiment 1 is that the amount of hydrogen peroxide added is adjusted to 4.8 mol.

[0108] Example 9 The difference between this embodiment and Embodiment 1 is that the amount of hydrogen peroxide added is adjusted to 3 mol.

[0109] Example 10 The difference between this embodiment and Embodiment 1 is that the molar amount of phosphate is adjusted to 6 mol.

[0110] Example 11 The difference between this embodiment and Embodiment 1 is that the molar amount of phosphate is adjusted to 11.25 mol.

[0111] Example 12 The difference between this embodiment and Embodiment 1 is that the molar amount of phosphate is adjusted to 12 mol.

[0112] Example 13 The difference between this embodiment and Embodiment 1 is that the molar amount of phosphate is adjusted to 5 mol.

[0113] Example 14 The difference between this embodiment and Embodiment 1 is that the temperature of the hydrothermal reaction is adjusted to 100°C.

[0114] Example 15 The difference between this embodiment and Embodiment 1 is that the temperature of the hydrothermal reaction is adjusted to 200°C.

[0115] Example 16 The difference between this embodiment and Embodiment 1 is that the temperature of the hydrothermal reaction is adjusted to 220°C.

[0116] Example 17 The difference between this embodiment and Embodiment 1 is that the temperature of the hydrothermal reaction is adjusted to 80°C.

[0117] Example 18 (1) At room temperature, iron oxide red (0.75 mol) and phosphoric acid solution (the mass fraction of phosphoric acid is 30% and the molar amount of phosphoric acid is 9.75 mol) are mixed and stirred evenly, and then added to a high-pressure reactor. The reaction is carried out at 100℃ for 2.5 h at a reaction pressure of 0.3 MPa. After the reaction is complete, the pressure is released to obtain the first mixture.

[0118] (2) Ferrous sulfate solution (21% ferrous sulfate by mass and 6.0 mol ferrous sulfate by molar amount) and hydrogen peroxide (27% hydrogen peroxide by mass and 3.6 mol hydrogen peroxide by molar amount) were added dropwise to the reactor at 20°C. The addition was completed in 30 min. Then the temperature of the reactor was set to 90°C and the stirring was continued for 80 min at a stirring rate of 100 r / min to obtain ferric phosphate dihydrate slurry.

[0119] (3) After solid-liquid separation, the ferric phosphate dihydrate slurry was rinsed until the conductivity of the washing liquid was ≤350μs / cm, then dried at 90℃ for 6h, and finally sintered at 550℃ for 4h to obtain anhydrous ferric phosphate.

[0120] Example 19 (1) At room temperature, iron oxide red (0.75 mol) and phosphoric acid solution (the mass fraction of phosphoric acid is 40% and the molar amount of phosphoric acid is 9.75 mol) are mixed and stirred evenly, and then added to a high-pressure reactor. The reaction is carried out at 200℃ for 1 h at a reaction pressure of 0.8 MPa. After the reaction is complete, the pressure is released to obtain the first mixture.

[0121] (2) Ferrous sulfate solution (21% ferrous sulfate by mass and 6.0 mol ferrous sulfate by molar amount) and hydrogen peroxide (28% hydrogen peroxide by mass and 3.6 mol hydrogen peroxide by molar amount) were added dropwise to the reactor at 30°C. The addition was completed in 10 min. Then the temperature of the reactor was set to 98°C and the stirring was continued for 30 min at a stirring rate of 200 r / min to obtain ferric phosphate dihydrate slurry.

[0122] (3) After solid-liquid separation, the ferric phosphate dihydrate slurry was rinsed until the conductivity of the washing liquid was ≤350μs / cm, then dried at 100℃ for 8h, and finally sintered at 700℃ for 2h to obtain anhydrous ferric phosphate.

[0123] Example 20 (1) At room temperature, iron oxide red (0.75 mol) and phosphoric acid solution (the mass fraction of phosphoric acid is 33.3% and the molar amount of phosphoric acid is 9.75 mol) are mixed and stirred evenly, and then added to a high-pressure reactor. The reaction is carried out at 80℃ for 1 h at a reaction pressure of 0.2 MPa. After the reaction is complete, the pressure is released to obtain the first mixture.

[0124] (2) Ferrous sulfate solution (21% ferrous sulfate by mass and 6.0 mol ferrous sulfate by molar amount) and hydrogen peroxide (27.5% hydrogen peroxide by mass and 3.6 mol hydrogen peroxide by molar amount) were added dropwise to the reaction vessel at 15°C. The addition was completed in 5 min. Then, the mixture was stirred at 85°C for 20 min at a stirring rate of 150 r / min to obtain ferric phosphate dihydrate slurry.

[0125] (3) After solid-liquid separation, the ferric phosphate dihydrate slurry was rinsed until the conductivity of the washing liquid was ≤350μs / cm, then dried at 80℃ for 5h, and finally sintered at 500℃ for 1h to obtain anhydrous ferric phosphate.

[0126] Example 21 (1) At room temperature, iron oxide red (0.75 mol) and phosphoric acid solution (the mass fraction of phosphoric acid is 33.3% and the molar amount of phosphoric acid is 9.75 mol) are mixed and stirred evenly, and then added to a high-pressure reactor. The reaction is carried out at 220℃ for 3 hours with a reaction pressure of 0.9 MPa. After the reaction is complete, the pressure is released to obtain the first mixture.

[0127] (2) Ferrous sulfate solution (21% ferrous sulfate by mass and 6.0 mol ferrous sulfate by molar amount) and hydrogen peroxide (27.5% hydrogen peroxide by mass and 3.6 mol hydrogen peroxide by molar amount) were added dropwise to the reactor at 40°C for 40 min. The addition was completed after 40 min. Then, the mixture was stirred at 100°C for 100 min at a stirring rate of 150 r / min to obtain ferric phosphate dihydrate slurry.

[0128] (3) After solid-liquid separation, the ferric phosphate dihydrate slurry was rinsed until the conductivity of the washing liquid was ≤350μs / cm, then dried at 120℃ for 10h, and finally sintered at 800℃ for 5h to obtain anhydrous ferric phosphate.

[0129] Comparative Example 1 The difference between this comparative example and Example 1 is that step (2) is omitted. The first mixture is separated into solid and liquid and then rinsed until the conductivity of the washing liquid is ≤350μs / cm. Then it is dried at 95℃ for 7h and finally sintered at 600℃ for 3h to obtain anhydrous iron phosphate.

[0130] Comparative Example 2 The difference between this comparative example and Example 1 is that step (1) is omitted. Phosphoric acid (mass fraction of phosphoric acid is 33.3%, molar amount of phosphoric acid is 9.75 mol), ferrous sulfate solution (mass fraction of ferrous sulfate is 21%, molar amount of ferrous sulfate is 6.0 mol) and hydrogen peroxide (mass fraction of hydrogen peroxide is 27.5%, molar amount of hydrogen peroxide is 3.6 mol) are added dropwise to the reaction vessel at 25°C. The addition is completed in 20 min. Then, the mixture is stirred at 95°C for 75 min at a stirring rate of 150 r / min to obtain ferric phosphate dihydrate slurry.

[0131] After solid-liquid separation, the ferric phosphate dihydrate slurry was rinsed until the conductivity of the washing liquid was ≤350μs / cm, then dried at 95℃ for 7h, and finally sintered at 600℃ for 3h to obtain anhydrous ferric phosphate.

[0132] II. Testing Methods (1) Property testing of cathode materials 1. XRD testing: The crystal structure of the iron phosphate material was characterized using an X-ray diffractometer (SmartLab SE) manufactured by Rigaku Corporation, Japan. The results are shown in [Figure number missing]. Figure 1 .

[0133] 2. SEM testing: The morphology of the iron phosphate material was characterized using a field emission scanning electron microscope (Sigma 500) manufactured by Zeiss AG, Germany. The results are shown in the figure below. Figures 2-9 .

[0134] 3. Element content: The content of each element in the iron phosphate material was tested using an inductively coupled plasma optical emission spectrometer (ICP-OES).

[0135] 4. BET specific surface area: determined by gas adsorption BET method.

[0136] 5. Compacted density: Tested using a compaction density meter with a test pressure of 3T and a compaction time of 30S.

[0137] 6. Tap density: Tested using a tap density meter with 5000 vibrations.

[0138] 7. Short axis length and long axis length of the rod-shaped structure of primary particles: Detected using SEM.

[0139] 8. D50 particle size: Detected using a laser particle size analyzer.

[0140] (ii) Properties of secondary batteries Preparation of lithium iron phosphate: Anhydrous iron phosphate prepared in each example and comparative example was mixed with lithium carbonate and glucose at a molar ratio of 1:0.525:0.07, and water was added to make a mixed slurry with a solid content of 41%. The slurry was then ground into a grinding slurry with a D50 particle size ≤1μm. The grinding slurry was then spray-dried to obtain a spray-dried material. The inlet air temperature of the spray drying was 210℃ and the outlet air temperature was 90℃. Finally, the spray-dried material was sintered at 750℃ for 10h under nitrogen protection, and then pulverized and packaged to obtain lithium iron phosphate.

[0141] Secondary battery assembly: Assembly of button cells: The above-mentioned lithium iron phosphate material is mixed with conductive agent (Super P, SP) and polyvinylidene fluoride in a mass ratio of 8:1:1 and added to N-methylpyrrolidone (NMP) to form a slurry. Then it is coated on aluminum foil, dried and pressed into sheets. Using lithium sheet as negative electrode, lithium hexafluorophosphate (LiPF6) as lithium salt, and ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) in a volume ratio of 1:1:1 as organic solvent, the lithium salt is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1M, and a button cell is prepared.

[0142] Battery performance testing: GB / T 42161-2022 Electrochemical performance testing of lithium iron phosphate, including test methods for first discharge specific capacity and first charge-discharge efficiency.

[0143] III. Analysis of Test Results for Each Embodiment and Comparative Example Table 1. Elemental analysis results of anhydrous ferric phosphate

[0144] Table 2. Detection results of size, tap density, and BET specific surface area of ​​anhydrous ferric phosphate.

[0145] Table 3 Electrochemical performance and compaction density results of lithium iron phosphate

[0146] Please see Figure 1 ,pass Figure 1 It can be seen that the anhydrous ferric phosphate prepared in the embodiments of this application are all monoclinic anhydrous ferric phosphate crystals with good crystallinity and no impurity peaks.

[0147] Please refer to Tables 1-3 and Figures 2-7 Through Table 1 and Figures 2-7 As can be seen, the anhydrous ferric phosphate material prepared in Examples 1-21 of this application comprises several secondary particles, which are spherical in shape and composed of several primary particles. The primary particles have a rod-like structure, with a major axis length of 4170 nm to 5200 nm and a minor axis length of 455 nm to 755 nm. The secondary particles are spherical with a D50 particle size of 3 μm to 6.5 μm. The tap density of this anhydrous ferric phosphate is 0.6 to 1.2 g / cm³. 3 BET has a specific surface area of ​​4m³. 2 / g~11m 2 / g; The compacted density of lithium iron phosphate prepared using the above-mentioned anhydrous ferric phosphate as a precursor is 2.3~2.5 g / cm³. 3 The initial charge capacity is 155mAh / g~166mAh / g, the initial discharge capacity is 149mAh / g~159mAh / g, and the initial coulombic efficiency is ≥93.7%.

[0148] Examples 1-5 show that when the molar ratio of iron oxide red to ferrous sulfate is 1:(3.7-9.6), especially 1:(4-9), the secondary particles of the anhydrous iron phosphate material have a more suitable D50 particle size and a narrower particle size distribution. The lithium iron phosphate cathode material prepared using the above-mentioned anhydrous iron phosphate as a precursor exhibits superior electrochemical performance. These results indicate that the molar ratio of iron oxide red to ferrous sulfate has a significant impact on the performance of the anhydrous iron phosphate material; both excessively high and excessively low molar ratios are detrimental to improving the performance of anhydrous iron phosphate.

[0149] A comparison of Examples 1 and 6-9 shows that when the molar ratio of ferrous sulfate to hydrogen peroxide is 1:(0.5~0.8), especially 1:(0.55~0.75), the secondary particles of the anhydrous iron phosphate material have a more suitable D50 particle size and a narrower particle size distribution. The lithium iron phosphate cathode material prepared using the above-mentioned anhydrous iron phosphate as a precursor exhibits superior electrochemical performance. These results indicate that the molar ratio of iron oxide red to phosphoric acid in the phosphoric acid solution has a significant impact on the performance of the anhydrous iron phosphate material; both excessively high and excessively low molar ratios of iron oxide red to phosphoric acid in the phosphoric acid solution are detrimental to improving the performance of anhydrous iron phosphate.

[0150] A comparison of Examples 1 and 10-13 shows that when the molar ratio of iron oxide red to phosphoric acid in the phosphoric acid solution is 1:(6.67-16), especially 1:(8-15), the secondary particles of the anhydrous iron phosphate material have a more suitable D50 particle size and a narrower particle size distribution. The lithium iron phosphate cathode material prepared using the above-mentioned anhydrous iron phosphate as a precursor exhibits superior electrochemical performance. These results indicate that the molar ratio of iron oxide red to phosphoric acid in the phosphoric acid solution has a significant impact on the performance of the anhydrous iron phosphate material; both excessively high and excessively low molar ratios are detrimental to improving the performance of anhydrous iron phosphate.

[0151] A comparison of Examples 1 and 14-17 shows that when the hydrothermal reaction temperature is 80-220℃, especially 100-200℃, the secondary particles of the anhydrous iron phosphate material have a more suitable D50 particle size and a narrower particle size distribution. The lithium iron phosphate cathode material prepared using the aforementioned anhydrous iron phosphate as a precursor exhibits superior electrochemical performance. These results indicate that the hydrothermal reaction temperature has a significant impact on the performance of the anhydrous iron phosphate material; excessively high or low temperatures are detrimental to improving the performance of anhydrous iron phosphate.

[0152] A comparison of Examples 1 and 20-21 shows that sintering temperatures of 550℃-700℃ and sintering times of 2h-4h result in a more suitable D50 particle size and narrower particle size distribution in the secondary particles of the anhydrous iron phosphate material. Consequently, the lithium iron phosphate cathode material prepared using the aforementioned anhydrous iron phosphate as a precursor exhibits superior electrochemical performance. These results demonstrate that the sintering temperature and time significantly influence the performance of the anhydrous iron phosphate material; excessively high or low sintering temperatures and times are detrimental to improving its performance.

[0153] A comparison between Example 1 and Comparative Example 1 shows that the D50 particle size of the anhydrous ferric phosphate secondary particles prepared in Comparative Example 1 is significantly higher than that of the examples in this application; and combined with Figures 8-9 It is known that the primary particles have a plate-like structure, while the secondary particles have a wide particle size distribution, which is not conducive to improving the discharge capacity, coulombic efficiency, and cycle life of lithium iron phosphate batteries.

[0154] A comparison between Example 1 and Comparative Example 2 shows that the D50 particle size and impurity element content of the anhydrous iron phosphate secondary particles prepared in Comparative Example 2 are higher than those in the examples of this application, which is not conducive to improving the discharge capacity, coulombic efficiency and cycle life of lithium iron phosphate batteries.

[0155] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. Anhydrous ferric phosphate, characterized in that, The primary particles of the anhydrous ferric phosphate have a rod-like structure, and the ratio of the length of the major axis to the length of the minor axis of the rod-like structure of the primary particles is (5.5~11.4):

1. The primary particle has a long axis length of 4170 nm to 5200 nm and a short axis length of 455 nm to 755 nm. The method for preparing the anhydrous ferric phosphate includes the following steps: Iron oxide and phosphoric acid solution are mixed and subjected to a first reaction treatment to obtain a first mixture. The temperature of the first reaction treatment is 100℃~200℃. The first mixture, ferrous salt and oxidant are mixed and subjected to a second reaction treatment to obtain ferric phosphate dihydrate slurry. The second reaction temperature is 90℃~98℃. The dihydrate ferric phosphate slurry was subjected to solid-liquid separation and sintering to obtain anhydrous ferric phosphate.

2. The anhydrous ferric phosphate according to claim 1, characterized in that, The secondary particles of the anhydrous ferric phosphate have a spherical morphology; and / or, The anhydrous iron phosphate has a D50 particle size of 3μm to 6.5μm.

3. The anhydrous ferric phosphate according to claim 1, characterized in that, The tap density of the anhydrous ferric phosphate is 0.6 g / cm³. 3 ~1.2g / cm 3 ; and / or, The anhydrous ferric phosphate has a BET specific surface area of ​​4 m². 2 / g~11m 2 / g; and / or, The anhydrous ferric phosphate has a Fe to P molar ratio of 0.955 to 0.99; and / or, The anhydrous iron phosphate has a monoclinic crystal form.

4. The anhydrous ferric phosphate according to claim 1, characterized in that, The molar ratio of the iron oxide to the phosphoric acid in the phosphoric acid solution is 1:(8~15); and / or, The phosphoric acid solution contains 30% to 40% phosphoric acid by mass; and / or, The pressure of the first reaction treatment is 0.3 MPa to 0.8 MPa, and the time of the first reaction treatment is 1 h to 2.5 h.

5. The anhydrous ferric phosphate according to claim 1, characterized in that, The ferrous salt is at least one of ferrous sulfate, ferrous chloride, or ferrous nitrate; and / or, The oxidant is at least one selected from hydrogen peroxide, sodium peroxide, potassium peroxide, sodium hypochlorite, potassium hypochlorite, sodium persulfate, potassium persulfate, and ozone; and / or, The molar ratio of the ferrous salt to the ferric oxide is (4~9):1; and / or, The molar ratio of the ferrous salt to the oxidant is 1:(0.5~0.8).

6. The anhydrous ferric phosphate according to claim 1, characterized in that, The step of mixing the first mixture, ferrous salt, and oxidant for a second reaction treatment to obtain ferric phosphate dihydrate slurry includes: The ferrous salt and the oxidant are mixed into the first mixture at a first mixing temperature for a first mixing time to obtain a second mixture; The second mixture is reacted at a second reaction temperature for a second reaction time to obtain ferric phosphate dihydrate slurry; in, The first mixing temperature is 20℃~30℃, and the first mixing time is 10min~30min; and / or, The second reaction time is 30 min to 80 min, and the second reaction treatment is carried out under stirring conditions.

7. The anhydrous ferric phosphate according to claim 1, characterized in that, The sintering temperature is 550℃~700℃, the sintering time is 2h~4h, and the sintering atmosphere is air.

8. A positive electrode material, characterized in that, The cathode material is lithium iron phosphate or lithium manganese iron phosphate prepared using anhydrous iron phosphate as a precursor as described in any one of claims 1 to 7.

9. A positive electrode sheet, characterized in that, The positive electrode sheet includes the positive electrode material as described in claim 8.

10. A secondary battery, characterized in that, The secondary battery includes the positive electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • Nanorod-shaped lithium iron phosphate material and preparation method thereof

    CN102945962A

  • Preparation method of battery-grade anhydrous iron phosphate

    CN112225190A

  • Iron phosphate dihydrate and preparation method thereof, iron phosphate, lithium iron phosphate and lithium ion battery

    CN114394581A

  • Iron phosphate as well as preparation method and application thereof

    CN118324108A