Preparation method and device of galvanic-effect-resistant copper foil with highly-enriched active metal on surface

By forming an electroplated thickening layer and a surface activation layer on the surface of copper foil, and utilizing the galvanic cell protection mechanism, the problem of galvanic etching of copper foil in silver solution is solved, avoiding burrs and bridging of PCB circuits, improving the copper foil's resistance to the galvanic effect, and ensuring the efficiency and quality of copper foil preparation.

CN120888996APending Publication Date: 2025-11-04VICTORY GIANT TECH HUIZHOU CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511077719.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-01
Publication Date
2025-11-04

AI Technical Summary

Technical Problem

In existing technologies, copper foil is prone to galvanic etching in silver solutions, leading to micro-short circuits such as burrs or bridging on PCB circuits. There is a lack of effective solutions to combat the galvanic effect.

Method used

The raw copper foil is thickened by cathodic electroplating on the bright surface using an electroplating electrolyte solution, and active metal ion electroplating is performed on the rough surface using an active metal mixed solution to form an electroplated thickening layer and a surface activation layer. This forms a galvanic cell on the copper foil surface to protect it and prevent the copper foil from reacting with silver ions.

Benefits of technology

It effectively avoids the galvanic etching reaction on the bottom of the copper foil, prevents the damage of micro short circuits caused by burrs or bridging of PCB circuits, and improves the efficiency and quality of copper foil preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120888996A_ABST
    Figure CN120888996A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of copper foil production, and particularly relates to a preparation method and device of a galvanic effect-resistant copper foil with highly-enriched active metal on the surface, and the preparation method comprises the following steps: carrying out cathode electroplating thickening on a raw material copper smooth surface by using an electroplating electrolytic solution, and forming an electroplating thickening layer on the surface of the raw material copper smooth surface; and performing active metal ion electroplating on the rough surface of the raw copper by using an active metal mixed solution to form a surface activation layer on the rough surface of the raw copper. According to the preparation method of the anti-galvanic-effect copper foil with the highly-enriched active metal on the surface, an electroplating thickening layer can be formed on the smooth surface of the raw copper, and a surface activation layer can be formed on the rough surface of the raw copper; therefore, the problem that galvanic corrosion reaction is easy to occur at the bottom of the copper foil due to the reaction of the existing copper foil and silver ions is solved, and the micro short circuit hazard of PCB circuit burrs or burr bridging caused by corrosion is effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of copper foil production, and particularly relates to a copper foil preparation method and device for resisting the Javelli effect of a surface with high enrichment of active metals. BACKGROUND

[0002] The Javelli effect, also known as galvanic corrosion or galvanic corrosion, refers to the phenomenon that when two different metals or alloys are in contact in an electrolyte solution, due to their different electrode potentials, an electrochemical cell effect is formed, thereby causing the corrosion / biting corrosion of the more active metal (anode). For example, when zinc Zn and copper Cu are in contact in an electrolyte solution, the potential of zinc is lower, and zinc becomes the anode; the potential of copper is higher, and copper becomes the cathode.

[0003] In general, chemical gold, OSP, tin spraying, and tin plating surface treatments will not cause the phenomenon of copper bottom biting corrosion; however, in the silver chemical solution system, due to the weak alkalinity of the chemical solution and the presence of organic conjugate bases, such as the reducing agent and organic matter commonly used in chemical silver deposition solution, including hydrazine hydrate, formaldehyde, grape sugar, tartrate, and dimethylamine borane, etc.; in addition, a large amount of free silver ions exist in the general chemical silver deposition solution, copper and the solution containing a large amount of free silver ions are prone to Cu+2Ag + →Cu 2+ displacement reaction, thereby causing the phenomenon of copper bottom biting corrosion.

[0004] In particular, the structure of large pads connecting small pads in PCBs, due to the difference in surface area between the two pads, the activation potential difference caused by the surface activation area, reduces the potential of the exposed large copper surface, causing the copper foil to have a lower potential, making it more prone to displacement reaction with the Ag + containing solution; especially as the surface silver deposition on the copper foil surface, the activation potential difference is more likely to attack from the copper tooth bottom of the copper foil and the substrate junction, aggravating the Javelli phenomenon of the copper bottom, thereby causing the copper foil circuit to have a micro-short circuit phenomenon of rough edges or rough edge bridging.

[0005] There is a blank in the prior art for the research of PCB copper foil bottom anti-Javelli effect, and there is an urgent need to research a technology that can effectively suppress the copper foil bottom biting corrosion to solve the problem of copper foil bottom biting corrosion in the silver chemical solution of PCB. SUMMARY

[0006] To solve the above problems, the first aspect of the application aims to provide a method for preparing copper foil with high surface enrichment of active metal to resist the Javelli effect, which combines cathode electroplating thickening of raw copper smooth surface by using electroplating electrolytic solution and active metal ion electroplating of raw copper rough surface by using active metal mixed solution; an electroplating thickening layer can be formed on the surface of the raw copper smooth surface, and a surface activation layer can be formed on the surface of the raw copper rough surface; when the copper foil is placed in silver water, the active metal in the surface activation layer can form a primary cell protection, thereby solving the problem that the existing copper foil reacts with silver ions and the Javelli corrosion reaction easily occurs at the bottom of the copper foil, effectively avoiding the PCB line edge or edge bridging micro-short circuit hazards caused by corrosion.

[0007] The second aspect of the application aims to provide a device for preparing copper foil with high surface enrichment of active metal to resist the Javelli effect, which is combined by a copper foil conveying mechanism, a copper foil electrolysis mechanism and a surface activation mechanism; not only can the raw copper smooth surface be cathode electroplated and thickened, and the raw copper rough surface be active metal ion electroplated, so as to form an electroplating thickening layer on the surface of the raw copper smooth surface and a surface activation layer on the surface of the raw copper rough surface, but also the copper foil conveying mechanism can continuously convey and turn over the raw copper during the preparation of the copper foil, effectively ensuring the efficiency of the preparation of the copper foil.

[0008] To achieve the above-mentioned purposes, the present application provides the following technical solutions: The method for preparing copper foil with high surface enrichment of active metal to resist the Javelli effect in the present application comprises the following steps: cathode electroplating thickening of raw copper smooth surface by using electroplating electrolytic solution to form an electroplating thickening layer on the surface of the raw copper smooth surface; active metal ion electroplating of raw copper rough surface by using active metal mixed solution to form a surface activation layer on the surface of the raw copper rough surface.

[0009] Further, the thickness of the raw copper is 2-6 μm; the thickness of the raw copper and the electroplating thickening layer is 12-35 μm; and the thickness of the surface activation layer is 0.2-2 μm.

[0010] Further, in the step of cathode electroplating thickening of raw copper smooth surface by using electroplating electrolytic solution to form an electroplating thickening layer on the surface of the raw copper smooth surface, the electroplating electrolytic solution is composed of the following components and component contents: The mass concentration of copper ions in the copper sulfate solution is 80-100 g / L The acid equivalent concentration (H + ) of the sulfuric acid solution is 1-2 mol / L Sodium dithiodipropyl sulfonate 0.02 g / L - 0.04 g / L Sodium phosphate monobasic 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01 g / L - 0.015 g / L.

[0011] Further, in the step of forming the electroplating thickening layer on the surface of the raw copper surface by cathode electroplating with the electroplating electrolytic solution, the current density is 400 A / m 2 - 800 A / m 2 .

[0012] Further, in the step of forming the surface activation layer on the surface of the raw copper surface by active metal ion electroplating with the active metal mixed solution, the active metal mixed solution is composed of the following components and component contents: Copper sulfate solution copper ion mass concentration is 50 g / L - 70 g / L Sulfuric acid solution acid equivalent concentration (H + ) is 2 mol / L - 4 mol / L Zinc sulfate zinc ion mass concentration is 0.8 g / L - 1.5 g / L Nickel nitrate nickel ion mass concentration is 0.2 g / L - 0.4 g / L Chromium trichloride chromium ion mass concentration is 0.05 g / L - 0.15 g / L Sodium dithiodipropyl sulfonate 0.02 g / L - 0.035 g / L Sodium phosphate monobasic 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01 g / L - 0.015 g / L Benzotriazole 0.16 g / L - 0.2 g / L.

[0013] Further, in the step of forming the surface activation layer on the surface of the raw copper surface by active metal ion electroplating with the active metal mixed solution, the current density is 100 A / m 2 - 600 A / m 2 .

[0014] Further, the electroplating thickness of the electroplating thickening layer and the surface activation layer is calculated by the following formula: ; Wherein, d is the electroplating thickness, M is the molar mass of the metal, D is the current density, t is the electroplating time, n is the charge number of the metal ion, F is the Faraday constant, and p is the metal density; That is, the electroplating thickening layer and the surface activation layer are calculated by the following formula: .

[0015] The device for preparing the copper foil with high enrichment of active metal and anti-Javan effect comprises: A copper foil conveying mechanism is used for winding, unwinding and conveying during the preparation of the copper foil; A copper foil electrolysis mechanism is used for cathode electroplating thickening of the raw copper surface to form an electroplating thickening layer on the surface of the raw copper surface; And a surface layer activation mechanism is used for active metal ion electroplating of the raw copper rough surface to form a surface activation layer on the surface of the raw copper rough surface.

[0016] Further, the copper foil conveying mechanism comprises: A raw copper unwinding assembly is arranged at the feeding end of the copper foil electrolysis mechanism and used for unwinding and conveying of the raw copper; A copper foil winding assembly is arranged at the discharging end of the surface layer activation mechanism and used for winding of the prepared copper foil; And an auxiliary roller assembly is arranged between the copper foil electrolysis mechanism and the surface layer activation mechanism and used for auxiliary conveying of the electroplated copper foil and electroplating surface replacement of the copper foil.

[0017] Further, the copper foil electrolysis mechanism comprises: A copper foil electrolysis tank; A copper foil cathode roller is arranged in the copper foil electrolysis tank and used for electroplating thickening and conveying of the raw copper surface; And the electroplating electrolytic solution as described above is arranged in the copper foil electrolysis tank and used for forming the electroplating thickening layer on the surface of the raw copper surface; The surface layer activation mechanism comprises: A surface layer activation cylinder; An activation layer processing cathode roller is arranged in the surface layer activation cylinder and used for active metal ion electroplating and conveying of the raw copper rough surface; And the active metal mixed solution as described above is arranged in the surface layer activation cylinder and used for forming the surface activation layer on the surface of the raw copper rough surface.

[0018] Based on the above technical solution, the present application has the following technical effects: 1. The copper foil with high surface enrichment of active metal and anti-Jarvan effect is prepared by the method, which comprises the following steps: cathode electroplating thickening of raw copper smooth surface by using electroplating electrolytic solution, and active metal ion electroplating of raw copper rough surface by using active metal mixed solution; the electroplating thickening layer is formed on the surface of the raw copper smooth surface, and the surface activation layer is formed on the surface of the raw copper rough surface; when the copper foil is placed in silver solution, the active metal in the surface activation layer can form a primary cell protection, thereby solving the problem that the copper foil reacts with silver ions and the bottom of the copper foil is prone to Jarvan corrosion, and effectively avoiding the micro-short circuit hazard caused by corrosion.

[0019] 2. The copper foil with high surface enrichment of active metal and anti-Jarvan effect is prepared by the device, which comprises a copper foil conveying mechanism, a copper foil electrolysis mechanism and a surface activation mechanism, and the copper foil is continuously conveyed and turned over in the process of copper foil preparation, so that the efficiency of copper foil preparation is effectively ensured. BRIEF DESCRIPTION OF DRAWINGS

[0020] Figure 1 The flow chart of the method for preparing the copper foil with high surface enrichment of active metal and anti-Jarvan effect is shown.

[0021] Figure 2 The overall structure schematic diagram of the device for preparing the copper foil with high surface enrichment of active metal and anti-Jarvan effect is shown.

[0022] Figure 3 The apparent structure image of the 1# copper foil sample observed under the microscope at a ratio of 1:1000 is shown.

[0023] Figure 4 The local section image of the 1# copper foil sample observed under the microscope at a ratio of 1:1000 is shown.

[0024] Figure 5 The apparent structure image of the 6# copper foil sample observed under the microscope at a ratio of 1:1000 is shown.

[0025] Figure 6 The apparent structure image of the 7# copper foil sample observed under the microscope at a ratio of 1:1000 is shown.

[0026] Figure 7 The apparent structure image of the 8# copper foil sample observed under the microscope at a ratio of 1:1000 is shown. DETAILED DESCRIPTION

[0027] For the purposes of the present application, the following terms shall have the meanings indicated below:

[0028] Before the various embodiments of the compounds / compositions and methods of the present disclosure are described in further detail, it is to be understood that this disclosure is not limited in its application to the details of construction and the arrangements of components set forth in the following description. The description provided herein is intended to be illustrative only and not restrictive; the inventive concept of the present disclosure is capable of being practiced with other embodiments and applied to various ways of making or using it. The language used in this document has been selected principally for readability. Thus, specific embodiments have been chosen for the purposes of explanation and understanding, and it is to be understood that the application is not limited to the specific embodiments described herein but includes all embodiments falling within the scope of the application. Furthermore, it is to be understood that the use of certain terms is for the purpose of explanation and understanding and is not to be taken as limiting.

[0029] However, it will be apparent to one of ordinary skill in the art that the embodiments of the present disclosure can be practiced without these specific details. In other instances, well-known features are not described in detail in order to avoid unnecessarily complicating the description. It is intended to include all alternatives, modifications, and equivalents falling within the scope of the present disclosure. All compounds / compositions disclosed herein can be prepared and used in accordance with the present disclosure without undue experimentation, in light of the present disclosure.

[0030] Thus, although the compounds / compositions and methods of the present disclosure have been described in accordance with specific embodiments, it is obvious that, based on the present disclosure, those skilled in the art can make modifications and alterations to the formulations, compounds or compositions and / or methods and the steps or order of steps in the methods described herein without departing from the spirit and scope of the inventive concept of the present disclosure.

[0031] As used herein, any reference to "one embodiment" or "the embodiment" means that a particular element, feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment. The appearances of the phrase "in one embodiment" in various places in the specification are not necessarily all referring to the same embodiment.

[0032] Unless otherwise defined herein, scientific and technical terms used in connection with the present disclosure shall have the meanings that are commonly understood by a person of ordinary skill in the art. Further, unless otherwise required by context, singular terms shall include pluralities and plural terms shall include the singular.

[0033] In a first aspect, referring to the accompanying drawings Figure 1 The present application provides a method for preparing copper foil with high surface enrichment of active metal and resistance to Javelli effect, comprising the following steps: S01, using electroplating electrolytic solution to perform cathode electroplating thickening on the raw copper smooth surface to form an electroplating thickening layer on the surface of the raw copper smooth surface; S02, using active metal mixed solution to perform active metal ion electroplating on the raw copper rough surface to form a surface activation layer on the surface of the raw copper rough surface.

[0034] The raw copper strip is an intermediate product in the production process of copper foil. It refers to a roll-shaped electroplated front traction copper foil or other conductive film, specifically including a copper foil or conductive film that meets the circumference of the copper foil cathode roller, such as a 3m diameter electroplating roller, with a length of 10 times the circumference, and a width equal to that of the copper foil cathode roller. Specifically, it can be a 2-6μm thick copper foil, a film (PET material) coated with a conductive material on the surface. That is, preferably, the thickness of the raw copper is 2-6μm; the thickness of the raw copper and the electroplating thickening layer is 12-35μm; and the thickness of the surface activation layer is 0.2-2μm.

[0035] In the chemical silver deposition solution, there are a large number of free silver ions, which are prone to Cu+2Ag + →Cu 2+ +2Ag displacement reaction; while in the gold solution, because gold ions generally exist in the form of chelate ligand, similar reactions do not occur. Therefore, in the presence of active alloy, because the copper particles are wrapped with other active metals, a kind of primary cell protection is formed, so that the copper foil is not easy to react with Ag + in the solution, and the problem of Javelli corrosion at the bottom of the copper foil is effectively avoided, which avoids the micro-short circuit hazard caused by corrosion and the PCB line edge or edge bridging.

[0036] Further, in the step of using electroplating electrolytic solution to perform cathode electroplating thickening on the raw copper smooth surface to form an electroplating thickening layer on the surface of the raw copper smooth surface, the electroplating electrolytic solution is composed of the following components and component contents: The mass concentration of copper ions in the copper sulfate solution is 80-100g / L The acid equivalent concentration (H + ) of the sulfuric acid solution is 1-2mol / L The concentration of polydithiobispropane sulfonic acid sodium is 0.02-0.04g / L Sodium phosphate dibasic 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01 g / L - 0.015 g / L.

[0037] In the step of forming the surface activation layer on the raw copper rough surface by electroplating with the active metal mixed solution, the active metal mixed solution is composed of the following components and component contents: Copper sulfate solution copper ion mass concentration is 50 g / L - 70 g / L Sulfuric acid solution acid equivalent concentration (H + ) is 2 mol / L - 4 mol / L Zinc sulfate zinc ion mass concentration is 0.8 g / L - 1.5 g / L Nickel nitrate nickel ion mass concentration is 0.2 g / L - 0.4 g / L Chromium trichloride chromium ion mass concentration is 0.05 g / L - 0.15 g / L Sodium polydithiopropanesulfonate 0.02 g / L - 0.035 g / L Sodium phosphate dibasic 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01 g / L - 0.015 g / L Benzotriazole 0.16 g / L - 0.2 g / L.

[0038] In electrochemistry, the activity order of metals can be judged by their standard electrode potentials. The lower the standard electrode potential, the higher the activity of the metal, that is, the easier the metal loses electrons and undergoes oxidation. The activity order of metals from high to low is: zinc (Zn) > nickel (Ni) > tin (Sn) > copper (Cu) > silver (Ag) > palladium (Pd) > gold (Au); In a large number of experiments, it is found that the earlier the active stripping component is added, the easier the primary cell protection is formed, the more the active metal is enriched on the rough surface of the copper foil (the contact surface with the compression resin), the better the anti-Javanian bite etching effect is, and the less the risk of etching notch is.

[0039] Further, in the step of forming the electroplating thickening layer on the raw copper smooth surface by cathode electroplating with the electroplating electrolytic solution, the current density is 400 A / m 2 -800 A / m 2 . In the step of forming the surface activation layer on the raw copper rough surface by electroplating with the active metal mixed solution, the current density is 100 A / m 2 -600 A / m 2 .

[0040] Further, the plating thickness of the plating thickening layer and the surface activation layer is calculated by the following formula: ; wherein d is the plating thickness, M is the molar mass of the metal, D is the current density, t is the plating time, n is the charge number of the metal ion, F is the Faraday constant, and p is the density of the metal. That is, the plating thickness calculation formula of the plating thickening layer and the surface activation layer is: .

[0041] The required plating thickness of the plating thickening layer and the surface activation layer can be achieved by adjusting the current density D and the plating time t.

[0042] In the second aspect, referring to the accompanying drawings, Figure 2 The application further provides a device for preparing the copper foil with high surface enrichment of active metal and resisting Javan effect, comprising: The copper foil conveying mechanism 10 is used for winding, unwinding and conveying during the preparation of the copper foil. The copper foil electrolysis mechanism 20 is used for cathode plating thickening on the raw copper smooth surface to form a plating thickening layer on the surface of the raw copper smooth surface. The surface activation mechanism 30 is used for active metal ion plating on the raw copper rough surface to form a surface activation layer on the surface of the raw copper rough surface.

[0043] Further, the copper foil conveying mechanism 10 comprises a raw copper unwinding assembly 11 arranged at the feeding end of the copper foil electrolysis mechanism 20 and used for unwinding and conveying the raw copper, a copper foil winding assembly 12 arranged at the discharging end of the surface activation mechanism 30 and used for winding the prepared copper foil, and an auxiliary roller assembly 13 arranged between the copper foil electrolysis mechanism 20 and the surface activation mechanism 30; the auxiliary roller assembly 13 is used for auxiliary conveying of the plating copper foil and plating surface replacement of the copper foil. Preferably, the auxiliary roller assembly 13 comprises a first auxiliary roller 131 arranged between the raw copper unwinding assembly 11 and the copper foil electrolysis mechanism 20, and a second auxiliary roller 132 arranged between the copper foil electrolysis mechanism 20 and the surface activation mechanism 30.

[0044] Further, the copper foil electrolysis mechanism 20 comprises a copper foil electrolysis tank 21; a copper foil cathode roller 22 arranged in the copper foil electrolysis tank 21 and used for plating thickening and conveying of the raw copper smooth surface, and a plating electrolysis solution 23 arranged in the copper foil electrolysis tank 21 and used for forming the plating thickening layer on the surface of the raw copper smooth surface, as described above.

[0045] The surface layer activation mechanism 30 comprises a surface layer activation cylinder 31; an activation layer processing cathode roller 32 arranged in the surface layer activation cylinder 31 and used for active metal ion electroplating delivery of a raw copper surface; and an active metal mixed solution 33 arranged in the surface layer activation cylinder 31 and used for forming a surface activation layer on the raw copper surface.

[0046] Embodiment: The embodiment provides a copper foil with a high enrichment of active metal and anti-Javan effect, and a preparation method thereof is as follows. S01, a raw copper unwinding assembly unwinds the raw copper, the raw copper passes through a first auxiliary roller assembly, is delivered to a copper foil cathode roller, and an electroplating electrolytic solution arranged in a copper foil electrolytic tank is used for cathode electroplating thickening of a raw copper surface, so that an electroplating thickening layer is formed on the raw copper surface.

[0047] The electroplating electrolytic solution is composed of the following components and component contents. The copper ion mass concentration of the copper sulfate solution is 80 g / L-100 g / L. The acid equivalent concentration (H + ) of the sulfuric acid solution is 1 mol / L-2 mol / L. The sodium dithionite is 0.02 g / L-0.04 g / L. The sodium dihydrogen phosphate is 0.01 g / L-0.015 g / L. The lauryl alcohol is 0.01 g / L-0.015 g / L. Preferably, the sodium dithionite is 0.03 g / L, the sodium dihydrogen phosphate is 0.012 g / L, and the lauryl alcohol is 0.012 g / L.

[0048] S02, the copper foil electroplated by the electroplating electrolytic solution is continuously delivered to an activation layer processing cathode roller, an active metal mixed solution arranged in a surface layer activation cylinder is used for active metal ion electroplating of a raw copper surface, and a surface activation layer is formed on the raw copper surface.

[0049] The active metal mixed solution is composed of the following components and component contents. The copper ion mass concentration of the copper sulfate solution is 50 g / L-70 g / L. The acid equivalent concentration (H + ) of the sulfuric acid solution is 2 mol / L-4 mol / L. The zinc ion mass concentration of the zinc sulfate is 0.8 g / L-1.5 g / L. The nickel ion mass concentration of the nickel nitrate is 0.2 g / L-0.4 g / L. The chromium ion mass concentration of the chromium trichloride is 0.05 g / L-0.15 g / L. Sodium polydithiopropyl sulfone 0.02 g / L - 0.035 g / L Sodium phosphate monobasic 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01 g / L - 0.015 g / L Benzotriazole 0.16 g / L - 0.2 g / L Preferably, the sodium polydithiopropyl sulfone is 0.025 g / L, the sodium phosphate monobasic is 0.012 g / L, the lauryl alcohol is 0.012 g / L, and the benzotriazole is 0.018 g / L.

[0050] Using the above preparation method, 1#-5# copper foil products were prepared respectively, and the main differences of each copper foil product are shown in Table 1.

[0051] Table 1 Differences of 1#-5# copper foil products

[0052] Comparative Example 1 A commercially available copper foil with a thickness of 18 μm, which has not been electroplated for thickening and active metal ion electroplating, was used as a 6# copper foil product.

[0053] Comparative Examples 2-7 Using the preparation method of the 3# copper foil product, 7#-12# copper foil products were prepared respectively, and the main differences are shown in Table 2.

[0054] Table 2 Differences of 7#-12# copper foil products

[0055] Test Example Copper foil morphology The 1#-5# copper foil products prepared in the examples and the 6#-12# copper foil products prepared in the comparative examples were respectively made into samples of vertical copper foil sections to prepare 1#-12# copper foil samples, and the copper tooth depth was observed as shown in Table 3; then the 1#-12# copper foil samples were treated with silver to observe whether there were copper wire burr phenomena at the bottom of the copper foil between the copper blocks with a spacing of 20 mil, and the observation results are shown in Table 3.

[0056] Table 3 Copper tooth depth and apparent morphology of 1#-12# copper foil samples after silver treatment

[0057] As shown in Table 3, the copper bite depth of the copper foil samples 1#-5# is basically below 5.2 μm, and the apparent morphology profile is clear; while the copper bite depth of the copper foil samples 7#-12# is basically above 5.7 μm, and the apparent morphology is rough with burrs. It can be seen that the copper foil product prepared by the preparation method in the application can effectively avoid the PCB line edge or edge bridging micro-short circuit hazard caused by bite.

[0058] Meanwhile, 1) The apparent image of the 1# copper foil is observed by a microscope at a ratio of 1:1000 as shown in FIG. 1, and the partial section image is as shown in FIG. 2; Figure 3 2) The apparent image of the 6# copper foil is observed by a microscope at a ratio of 1:1000 as shown in FIG. 3; Figure 4 3) The apparent image of the 7# copper foil is observed by a microscope at a ratio of 1:1000 as shown in FIG. 4; 4) The apparent image of the 8# copper foil is observed by a microscope at a ratio of 1:1000 as shown in FIG. 5. Figure 5 By comparison, Figure 6 the apparent image profile of the 1#-5# copper foil is clear without burrs, the partial section image of the 6#-8# copper foil forms a complete etching trapezoid at the bottom of the copper foil cross section; while Figure 7 the apparent image of the 7#-12# copper foil has obvious rough burrs. It can be seen that the copper foil product prepared by the preparation method in the application can effectively solve the problem of the existing copper foil and silver ion reaction, the copper foil bottom is prone to Gavani bite reaction, and effectively avoid the PCB line edge or edge bridging micro-short circuit hazard caused by bite.

[0059] By comparison of Table 3, Figure 3 it can be seen that when the active metal mixed solution with low zinc ion concentration is used to prepare the copper foil, the significant Gavani corrosion phenomenon occurs; and by comparison of Figure 4 it can be seen that when the active metal mixed solution with zinc ion mass concentration exceeding 1.5 g / L is used to prepare the copper foil, the obvious Gavani corrosion phenomenon also occurs. It can be seen that the copper foil prepared by the active metal mixed solution with the preset active metal ion mass concentration in the application can effectively solve the problem of the existing copper foil and silver ion reaction, the copper foil bottom is prone to Gavani bite reaction, and effectively avoid the PCB line edge or edge bridging micro-short circuit hazard caused by bite. Figure 5-7

[0060] Figure 3 Figure 6 Figure 3 7

[0061] ​​​​​​​The above merely illustrates and describes the structure of the present application, and the description is relatively specific and detailed, but should not be understood as a limitation on the scope of the present application. It should be noted that, for those skilled in the art, without departing from the concept of the present application, several modifications and improvements can be made, and these obvious replacement forms all belong to the protection scope of the present application.

Claims

1. A method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect, characterized in that, Includes the following steps: A cathode electroplating thickening method is used to thicken the raw copper bright surface by electroplating with an electroplating electrolyte solution, thereby forming an electroplated thickening layer on the surface of the raw copper bright surface. Active metal ion electroplating is performed on the raw copper rough surface using an active metal mixed solution to form a surface activation layer on the surface of the raw copper rough surface.

2. The method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect according to claim 1, characterized in that, The thickness of the raw copper is 2μm-6μm; the overall thickness of the raw copper and the electroplated thickened layer is 12μm-35μm; and the thickness of the surface activation layer is 0.2μm-2μm.

3. The method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect according to claim 1, characterized in that, In the step of using an electroplating electrolyte solution to perform cathodic electroplating to thicken the raw copper surface, and forming an electroplated thickened layer on the surface of the raw copper surface, the electroplating electrolyte solution consists of the following components and their contents: The copper ion concentration in the copper sulfate solution is 80 g / L - 100 g / L. Sulfuric acid solution acid equivalent concentration (H) + (1 mol / L - 2 mol / L) Sodium polydisulfide dipropane sulfonate 0.02 g / L - 0.04 g / L Sodium dihydrogen phosphate 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01g / L - 0.015g / L.

4. The method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect according to claim 1, characterized in that, In the step of using an electroplating electrolyte to perform cathodic electroplating to thicken the raw copper surface, and forming the thickened electroplated layer on the surface of the raw copper surface, the current density is 400 A / m. 2 -800A / m 2 .

5. The method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect according to claim 1, characterized in that, In the step of forming a surface activation layer on the raw copper rough surface by electroplating with an active metal mixed solution, the active metal mixed solution consists of the following components and their contents: The copper ion concentration in the copper sulfate solution is 50 g / L - 70 g / L. Sulfuric acid solution acid equivalent concentration (H) + (2 mol / L - 4 mol / L) The zinc ion concentration of zinc sulfate is 0.8 g / L - 1.5 g / L. The nickel ion concentration of nickel nitrate is 0.2 g / L - 0.4 g / L. The chromium ion concentration of chromium trichloride is 0.05 g / L - 0.15 g / L. Sodium polydisulfide dipropane sulfonate 0.02 g / L - 0.035 g / L Sodium dihydrogen phosphate 0.01 g / L - 0.015 g / L Lauryl alcohol 0.01 g / L - 0.015 g / L Benzotriazole 0.16 g / L - 0.2 g / L.

6. The method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect according to claim 1, characterized in that, In the step of forming a surface activation layer on the raw copper rough surface using an active metal mixed solution, the current density is 100 A / m. 2 -600A / m 2 .

7. The method for preparing copper foil with highly enriched active metals on the surface to resist the Gabriel effect according to claim 1, characterized in that, The electroplating thickness of the electroplated thickening layer and the surface activation layer are calculated using the following formula: ; Where d is the electroplating thickness, M is the molar mass of the metal, D is the current density, t is the electroplating time, n is the charge number of the metal ions, F is the Faraday constant, and ρ is the metal density. That is, the formulas for calculating the electroplating thickness of the thickened layer and the surface activation layer are as follows: 。 8. An apparatus for preparing copper foil with highly enriched active metals on the surface to resist the galvanic effect as described in any one of claims 1-7, characterized in that, include: A copper foil conveying mechanism is used for winding, unwinding, and conveying during the copper foil preparation process. A copper foil electrolysis mechanism is used to perform cathode electroplating to thicken the raw copper surface, forming an electroplated thickened layer on the surface of the raw copper surface; And a surface activation mechanism for performing active metal ion electroplating on the raw copper rough surface to form a surface activation layer on the surface of the raw copper rough surface.

9. The apparatus for preparing copper foil with high surface enrichment of active metals to resist the Gabriel effect according to claim 8, characterized in that, The copper foil conveying mechanism includes: A raw copper unwinding assembly is installed at the feed end of the copper foil electrolysis mechanism for unwinding and conveying raw copper. A copper foil winding assembly is provided at the discharge end of the surface activation mechanism for winding the copper foil after preparation. An auxiliary roller assembly is provided between the copper foil electrolysis mechanism and the surface activation mechanism for auxiliary conveying of the electroplated copper foil and for changing the electroplating surface of the copper foil.

10. The apparatus for preparing copper foil with high surface enrichment of active metals to resist the Gabriel effect according to claim 8, characterized in that, The copper foil electrolysis mechanism includes: Copper foil electrolytic cell; A copper foil cathode roller is installed inside the copper foil electrolytic cell for conveying raw copper foil to thicken its electroplating surface. And the electroplating solution as described in claim 1 or 3, disposed in the copper foil electrolytic cell, to achieve the formation of an electroplated thickened layer on the surface of the raw copper. The surface activation mechanism includes: Surface activation tank; The activation layer processing cathode roller is set inside the surface activation cylinder and is used for the electroplating of active metal ions on the raw copper rough surface. And the active metal mixed solution as described in claim 1 or 5, disposed in the surface activation tank, to achieve the formation of a surface activation layer on the raw copper rough surface.