Positive electrode particle and preparation method thereof, positive electrode plate and sodium battery

By designing a gradient-increasing porosity distribution for cathode particles and a method for preparing a carbon coating layer, the problems of insufficient compaction density and rate performance of sodium iron pyrophosphate in sodium batteries were solved, achieving improved high energy density and kinetic performance.

CN120895651AActive Publication Date: 2025-11-04XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511061975.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-30
Publication Date
2025-11-04
Estimated Expiration
2045-07-30

AI Technical Summary

Technical Problem

In existing technologies, sodium iron pyrophosphate is difficult to achieve both high compaction density and high rate performance, which affects the energy density and kinetic performance of sodium batteries.

Method used

A positive electrode particle is designed with a gradient increase in porosity on its maximum cross-section, gradually increasing from the inside to the outside. The secondary particles of sodium iron pyrophosphate are coated with a carbon layer by a preparation method to form inner, middle and outer layers with porosities of P1, P2 and P3, respectively, satisfying the relationship P1 < P2 < P3.

Benefits of technology

This improved the compaction density of the cathode particles and the wettability of the electrolyte, thereby enhancing the energy density and kinetic performance of the sodium battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120895651A_ABST
    Figure CN120895651A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode particle and a preparation method thereof, a positive electrode plate and a sodium battery. The positive electrode particle provided by the invention has a first porosity P1 in the range of 1 / 2 radius on the maximum cross section, a second porosity P2 in the range of 1 / 2 radius to 3 / 4 radius on the maximum cross section of the positive electrode particle, and a third porosity P3 in the range of 3 / 4 radius on the maximum cross section of the positive electrode particle to the surface of the positive electrode particle, P1 < P2 < P3, and P1 < P2 < P3. And the maximum cross section of the positive electrode particle refers to the cross section where the maximum length direction of the positive electrode particle is located.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of batteries, in particular to a positive electrode particle and a preparation method thereof, a positive electrode sheet and a sodium battery. BACKGROUND

[0002] Sodium batteries are considered as a promising large-scale energy storage solution due to their abundant sodium resources, wide distribution and low cost. In recent years, they have received widespread attention. Sodium iron pyrophosphate Na4Fe3(PO4)2P2O7, which has a three-dimensional sodium ion diffusion channel and a sodium superionic conductor structure, has the characteristics of high voltage platform, high capacity, excellent rate and cycle stability, and has great potential to become a large-scale production positive electrode material for sodium batteries. However, in the related art, sodium iron pyrophosphate is difficult to have both high tap density and high rate performance. SUMMARY

[0003] The embodiments of the present application provide a positive electrode particle having high tap density and high rate performance.

[0004] In a first aspect, the embodiments of the present application provide a positive electrode particle, the positive electrode particle having a first porosity P1 within a 1 / 2 radius range on a maximum cross section of the positive electrode particle, the positive electrode particle having a second porosity P2 between a 1 / 2 radius and a 3 / 4 radius on the maximum cross section of the positive electrode particle, and the positive electrode particle having a third porosity P3 between the 3 / 4 radius and a surface of the positive electrode particle on the maximum cross section of the positive electrode particle, wherein P1

[0005] In some embodiments, the porosity on the maximum cross section of the positive electrode particle gradually increases from inside to outside along a radial direction.

[0006] In some embodiments, the average porosity P of the maximum cross section of the positive electrode particle ranges from 5% to 30%.

[0007] In some embodiments, the first porosity P1 ranges from 3% to 15%.

[0008] In some embodiments, the second porosity P2 ranges from 7% to 18%.

[0009] In some embodiments, the third porosity P3 ranges from 10% to 28%.

[0010] In some embodiments, the maximum cross section of the positive electrode particle satisfies at least one of the following relationships:

[0011] (5P2+7P3) / P1>12; and

[0012] (4P1+5P2) / P3<9.

[0013] In some embodiments, the positive electrode particle is a sodium iron phosphate pyrophosphate secondary particle, the sodium iron phosphate pyrophosphate secondary particle is composed of a plurality of sodium iron phosphate pyrophosphate primary particles; the chemical formula of the sodium iron phosphate pyrophosphate is: Na x Fe y Me z (PO4) α (P2O7) β , wherein Me is at least one of Mg, Ca, Al, Ti, V, Mn, Cr, Cu, Zn, Zr, Nb, W, Mo, Sc, Y, 3.7≤x≤4.3, 2.8≤y+z≤3.0, 0≤z≤1.0, 3.9≤α+2β≤4.1.

[0014] In some embodiments, the positive electrode particle is a sodium iron phosphate pyrophosphate secondary particle, the sodium iron phosphate pyrophosphate secondary particle is composed of a plurality of sodium iron phosphate pyrophosphate primary particles; the sodium iron phosphate pyrophosphate primary particle comprises an active inner core and a carbon layer, the active inner core is sodium iron phosphate pyrophosphate, the carbon layer is wrapped on the surface of the active inner core, and the mass fraction of the carbon layer in the positive electrode particle ranges from 1.0wt% to 3.0wt%.

[0015] In a second aspect, the embodiments of the present application provide a preparation method of a positive electrode particle, the preparation method comprises:

[0016] providing a sodium source, a phosphorus source, an iron source and a carbon source;

[0017] putting the sodium source, the phosphorus source, the iron source and the carbon source into a solvent for sand milling to obtain a slurry;

[0018] spray drying the slurry to obtain a precursor powder; and

[0019] sequentially pre-sintering and sintering the precursor powder to obtain the positive electrode particle, wherein the positive electrode particle has a first porosity P1 within a 1 / 2 radius range on a maximum cross section of the positive electrode particle, the positive electrode particle has a second porosity P2 between the 1 / 2 radius and a 3 / 4 radius on the maximum cross section of the positive electrode particle, and the positive electrode particle has a third porosity P3 between the 3 / 4 radius and a surface of the positive electrode particle on the maximum cross section of the positive electrode particle, wherein P1

[0020] In some embodiments, the slurry comprises solid particles, and a volume median particle size Dv50 of the solid particles ranges from 100nm≤Dv50≤300nm.

[0021] In some embodiments, the sequentially pre-sintering and sintering the precursor powder to obtain the positive electrode particles comprises:

[0022] pre-sintering the precursor powder at a first temperature increasing rate to 250-400 DEG C to obtain an intermediate; and

[0023] sintering the intermediate at a second temperature increasing rate to 500-650 DEG C to obtain the positive electrode particles.

[0024] In some embodiments, the first temperature increasing rate ranges from 2 DEG C / min to 10 DEG C / min; and the second temperature increasing rate ranges from 1 DEG C / min to 5 DEG C / min.

[0025] In a third aspect, the embodiments of the present application provide a positive electrode tab, comprising:

[0026] a positive electrode current collector; and

[0027] a positive electrode active layer comprising the positive electrode particles according to the embodiments of the present application.

[0028] In a fourth aspect, the embodiments of the present application provide a sodium battery, comprising: an electrolyte, the positive electrode tab according to the embodiments of the present application, a separator, and a negative electrode tab.

[0029] The cathode particle in this embodiment has a first porosity P1 within half the radius of its maximum cross-section, a second porosity P2 between half and three-quarters of its maximum cross-section, and a third porosity P3 between three-quarters of its maximum cross-section and the surface of the cathode particle, wherein P1 < P2 < P3, and the maximum cross-section of the cathode particle refers to the cross-section along its maximum length direction. This application achieves a gradient increase in pore size from the inside to the outside of the cathode particle, resulting in a lower overall porosity and higher compaction density, thus enabling the sodium battery to have a higher energy density. Furthermore, the pore size distribution exhibits a gradient increase from the inside out, resulting in a higher pore size, larger specific surface area, and greater roughness on the surface of the cathode particles. This facilitates electrolyte wetting of the cathode particles, improving their electrolyte wettability. Moreover, the pore structure with a decreasing porosity gradient from the outside in allows the electrolyte to gradually penetrate the interior of the cathode particles through capillary action after initial surface wetting. This ensures that even the lower porosity areas within the cathode particles are well wetted by the electrolyte, resulting in excellent electrolyte wettability and thus improved kinetic and rate performance of the sodium battery. In summary, this application, through its design of a gradient increase in porosity from the inside out, achieves a high powder compaction density in the cathode particles, enabling the sodium battery to possess both high energy density and excellent kinetic and rate performance. Attached Figure Description

[0030] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0031] Figure 1 This is a schematic diagram of the structure of an energy storage system according to an embodiment of this application.

[0032] Figure 2 This is a schematic diagram of the structure of an energy storage system according to another embodiment of this application.

[0033] Figure 3 This is a schematic diagram of the structure of an energy storage device according to an embodiment of this application.

[0034] Figure 4 This is a schematic diagram of the structure of a sodium battery according to an embodiment of this application.

[0035] Figure 5 For the application of an embodiment of a sodium battery Figure 4A-A direction cross-sectional structure schematic view.

[0036] Figure 6 A cross-sectional view of a negative electrode plate according to an embodiment of the application.

[0037] Figure 7 A cross-sectional view of a positive electrode plate according to an embodiment of the application.

[0038] Figure 8 A structure schematic view of a positive electrode particle according to an embodiment of the application.

[0039] Figure 9 A structure schematic view of a positive electrode particle according to another embodiment of the application.

[0040] Figure 10 A flowchart of a preparation method of a positive electrode particle according to an embodiment of the application.

[0041] Figure 11 A flowchart of pre-sintering and sintering in a preparation method of a positive electrode particle according to an embodiment of the application.

[0042] Explanation of reference signs:

[0043] 100 - energy storage system, 110 - high-voltage cable, 120 - first electric energy conversion device, 130 - second electric energy conversion device, 140 - third electric energy conversion device, 150 - first user load, 160 - second user load, 200 - energy storage device, 210 - single battery, 300 - sodium battery, 320 - diaphragm, 330 - negative electrode plate, 331 - negative electrode current collector, 332 - negative electrode active layer, 340 - shell, 350 - end cover assembly, 400 - positive electrode plate, 410 - positive electrode current collector, 420 - positive electrode active layer, 500 - positive electrode particle, 510 - pore, 520 - sodium iron pyrophosphate primary particle, 521 - active core, 522 - carbon layer. DETAILED DESCRIPTION

[0044] In order to enable persons skilled in the art to better understand the schemes of the present application, the technical schemes in the embodiments of the present application will be described clearly and completely below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only some of the embodiments of the present application, but not all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by persons skilled in the art without creative labor fall within the scope of protection of the present application.

[0045] The terms "first", "second", etc. in the specification and claims of the present application and in the above drawings are used to distinguish different objects, and are not used to describe a particular order. In addition, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusion. For example, a process, method, system, product or device including a series of steps or units is not limited to the listed steps or units, but can optionally include steps or units not listed, or can optionally include other steps or units inherent to the process, method, product or device.

[0046] The technical solutions in the embodiments of the present application will be described below with reference to the drawings.

[0047] It should be noted that, for the sake of illustration, in the embodiments of the present application, the same reference signs represent the same parts, and for the sake of brevity, detailed descriptions of the same parts are omitted in different embodiments.

[0048] Since the energy required by people has strong time and space characteristics, in order to reasonably use energy and improve the utilization rate of energy, it is necessary to store one form of energy in the same form or convert it into another form of energy through a medium or device, and release it in a specific energy form based on future application needs. At present, the main way to generate green electricity is to develop photovoltaic, wind power and other green energy to replace fossil energy.

[0049] At present, the generation of green electricity generally relies on photovoltaic, wind power, water potential, etc., while wind energy and solar energy have strong intermittency and large fluctuation, which can cause unstable power grid, insufficient electricity at peak demand, too much electricity at low demand, and unstable voltage which can damage power. Therefore, due to insufficient electricity demand or insufficient grid acceptance capacity, the problem of "abandoning wind and light" may occur. To solve these problems, energy storage is needed. That is, the electrical energy is converted into other forms of energy through physical or chemical means and stored, and the energy is converted into electrical energy and released when needed. In simple terms, energy storage is similar to a large "power bank", which stores electrical energy when photovoltaic and wind energy is sufficient, and releases the stored electrical energy when needed.

[0050] Taking electrochemical energy storage as an example, the present scheme provides an energy storage device applied to an energy storage system, which is internally provided with a group of chemical batteries, mainly using chemical elements in the batteries as energy storage medium. The charging and discharging process is accompanied by chemical reaction or change of the energy storage medium. In simple terms, the electrical energy generated by wind and solar energy is stored in the chemical battery, and the stored electrical energy is released for use when the use of external electrical energy reaches the peak, or is transferred to a place where electrical energy is in short supply for use.

[0051] Current energy storage applications are widely used, including energy storage on the power generation side, the power grid side and the power consumption side. The corresponding energy storage devices include:

[0052] (1) Large-scale energy storage power stations applied in wind power and photovoltaic power stations can help renewable energy generation to meet grid connection requirements and improve renewable energy utilization. As high-quality active / reactive power regulation power sources on the power supply side, energy storage power stations can realize load matching in time and space, enhance renewable energy consumption capacity, reduce instantaneous power changes, reduce the impact on the power grid, and improve new energy power generation consumption and have great significance in power grid system backup, peak load power supply pressure relief and peak regulation;

[0053] (2) Energy storage containers applied in the power grid side mainly function in peak regulation, frequency regulation and congestion relief. They can realize peak load shaving and valley filling, i.e., charging energy storage batteries when the power load is low and releasing stored power when the power load is high, thereby balancing power production and consumption;

[0054] (3) Small energy storage cabinets applied in the power consumption side mainly function in power self-generation and self-use, peak-valley price arbitrage, capacity cost management and improvement of power supply reliability. According to different application scenarios, power consumption side energy storage can be divided into industrial and commercial energy storage cabinets, household energy storage devices and energy storage charging piles, which are generally used with distributed photovoltaic power. Industrial and commercial users can use energy storage for peak-valley price arbitrage and capacity cost management. In the electricity market implementing peak-valley electricity prices, the energy storage system is charged at low prices and discharged at high prices to realize peak-valley price arbitrage and reduce electricity costs. In addition, industrial enterprises using two-part electricity prices can use the energy storage system to store energy during low power consumption and discharge during peak load, thereby reducing peak power and the maximum demand amount reported, achieving the purpose of reducing capacity electricity costs. Household photovoltaic power with storage can improve the level of power self-generation and self-use. Due to high electricity prices and poor power supply stability, household photovoltaic power demand is driven. Considering that photovoltaic power is generated during the day and users generally have high load at night, the configuration of energy storage can better utilize photovoltaic power, improve the level of self-generation and self-use, and reduce electricity costs. In addition, communication base stations and data centers need to be equipped with energy storage for backup power.

[0055] In some embodiments, referring to Figure 1 , Figure 1 FIG. 1 is a structural schematic diagram of an energy storage system 100 according to an embodiment of the present application, and the energy storage system 100 according to the embodiment of the present application is not limited to the energy storage scenario of the power generation and distribution side. Figure 1 The embodiment of the present application is described by taking the power generation and distribution side shared energy storage scenario as an example, and the energy storage device 200 according to the present application is not limited to the power generation and distribution side energy storage scenario.

[0056] The application provides a kind of energy storage system 100, the energy storage system 100 includes: high voltage cable 110, first electric energy conversion device 120, second electric energy conversion device 130 and the energy storage device 200 provided by the application, in some embodiments of power generation side scene, second electric energy conversion device 130 can be wind power electric energy conversion device, due to the fluctuation, randomness and intermittence of wind power electric energy conversion generated electric energy, unstable electric energy output by wind power electric energy conversion device can be stored to energy storage device 200 by grid connection first, energy storage device 200 is connected with high voltage cable 110 and exports smooth electric energy to supply distribution network for use, realize peak shaving and frequency modulation, grid stable operation;Or, wind power electric energy conversion device is always connected with high voltage cable 110, and the electric energy output by wind power electric energy conversion device is supplied to distribution network for use by high voltage cable 110 in ordinary power generation, and when current power load is low, wind power electric energy conversion device generates excess, first store the electric quantity of overproduction to energy storage device 200, reduce the rate of wind curtailment and light curtailment, improve new energy power generation consumption problem;And when power load is high, grid issues an order, and the electric quantity stored in energy storage device 200 is transmitted to power side for use by grid connection mode with high voltage cable 110, provides peak shaving, frequency modulation, backup and other services for grid operation, fully plays the role of grid peak shaving, promotes grid peak clipping, and relieves grid power supply pressure.

[0057] In some embodiments of distribution network side, first electric energy conversion device 120 can be photovoltaic electric energy conversion device, energy storage device 200 is connected with high voltage cable 110 and is installed between downstream of high voltage cable 110 and user load, and the electric energy output by photovoltaic electric energy conversion device is stored in energy storage device 200, which can be used as backup power source in time when grid / distribution network fails;Or, when high voltage cable 110 transmission line appears line congestion, provide power support to delay economic pressure generated by grid / distribution expansion.

[0058] Optionally, first electric energy conversion device 120 can include but is not limited to wind power electric energy conversion device, and second electric energy conversion device 130 can include but is not limited to photovoltaic electric energy conversion device, and the first electric energy conversion device 120 and the second electric energy conversion device 130 can convert at least one of solar energy, light energy, wind energy, heat energy, tidal energy, biomass energy and mechanical energy into electric energy.

[0059] In some embodiments, please refer to Figure 2 , Figure 2 The structure schematic diagram of the energy storage system 100 of another embodiment of the application is provided, and the energy storage device 200 of the application Figure 2 Embodiments take household energy storage scene in user side energy storage as an example for illustration, and the energy storage device 200 of the application is not limited to household energy storage scene.

[0060] The application provides a kind of energy storage system 100, the energy storage system 100 includes third electric energy conversion device 140 (for example photovoltaic panel), first user load 150 (household lamps and lanterns), second user load 160 (such as air conditioner and household appliances) and so on and energy storage device 200, the energy storage device 200 is small energy storage box, can be installed in outdoor wall by wall hanging mode, the energy storage device 200 of the application is not limited to wall hanging mode, can also be placed in user residence by other ways.For specific, photovoltaic panel can convert solar energy into electric energy in the period of low electricity price, the energy storage device 200 is used to store the electric energy and supply lamps and lanterns and household appliances for use in the period of high electricity price, or power supply when power grid is disconnected / power off.

[0061] Optionally, the energy storage device 200 can include but is not limited to energy storage application scenarios such as energy storage power station, hydroelectric power / thermal power / wind power generation system, solar power generation system, mobile power system, smart home system or temporary power supply system, and is also applied to data centers, military equipment, aerospace, charging piles, electric vehicles and other fields.

[0062] Please see Figure 3 , Figure 3 The structure schematic diagram of the energy storage device 200 of an embodiment of the application.

[0063] Optionally, the energy storage device 200 can include but is not limited to one or more single batteries 210.

[0064] The term "a plurality of" means greater than or equal to two, for example, can be but is not limited to 2, 5, 10, 30, 50, 100, 200, 300, 400, 800, 1000 and the like.The number of single batteries 210 included in the energy storage device 200 can be determined according to the rated capacity of the single battery 210 and the rated capacity to be achieved by the energy storage device 200.

[0065] It should be noted that when the energy storage device 200 includes one single battery 210, the energy storage device 200 can exist in the form of the single battery 210.When the energy storage device 200 includes a plurality of single batteries 210, the plurality of single batteries 210 can be arranged by stacking, assembled and the like, to form a battery module, a battery pack, a battery cluster, a mobile power supply, an energy storage cabinet / energy storage container and other battery integrated systems.In other words, the energy storage device 200 can be but is not limited to exist in the form of a battery module, a battery pack, a battery cluster, a mobile power supply, an energy storage cabinet / energy storage container and other battery integrated systems.The actual application form of the energy storage device 200 provided in the embodiments of the application can be but is not limited to the listed products, and can also be other application forms, and the embodiments of the application do not strictly limit the application form of the energy storage device 200.The embodiments of the application only take the energy storage device 200 as a multi-core battery as an example for description.

[0066] Optionally, the single cell 210 can be, but is not limited to, at least one of cylindrical, square, prismatic, or other shaped cells.

[0067] Optionally, the single cell 210 can be a rechargeable battery, which refers to a single cell 210 that can be recharged after discharge to activate the active materials and continue to be used. The single cell 210 can be a lithium-ion battery, sodium-ion battery, sodium-lithium-ion battery, lithium metal battery, sodium metal battery, lithium-sulfur battery, magnesium-ion battery, nickel-metal hydride battery, nickel-cadmium battery, lead-acid battery, etc., and this application does not specifically limit it.

[0068] Understandably, the single cell 210 can be, but is not limited to, a sodium battery 300, a lithium battery, a magnesium battery, a nickel-metal hydride battery, a nickel-cadmium battery, a lead-acid battery, etc. In the following embodiments of this application, the single cell 210 is illustrated using a sodium battery 300 as an example.

[0069] Sodium batteries, with their advantages of abundant and widely distributed sodium resources and low cost, are considered a highly promising large-scale energy storage solution and have received widespread attention in recent years. Sodium iron pyrophosphate (Na4Fe3(PO4)2P2O7), possessing a three-dimensional sodium ion diffusion channel and a sodium superionic conductor structure, exhibits high voltage plateau, high capacity, excellent rate capability, and excellent cycle stability, making it a very promising cathode material for large-scale production in sodium batteries. However, in related technologies, sodium iron pyrophosphate has struggled to simultaneously achieve both high compaction density and high rate performance.

[0070] Therefore, embodiments of this application provide a positive electrode particle and its preparation method, a positive electrode sheet, and a sodium battery.

[0071] Figure 4 This is a schematic diagram of the structure of a sodium battery 300 according to an embodiment of this application. Figure 5 For the application of an embodiment of a sodium battery 300 along Figure 4 A schematic diagram of the cross-sectional structure along the AA direction.

[0072] Please see Figure 4 and Figure 5 This application also provides a sodium battery 300, which includes an electrolyte, a positive electrode 400, a separator 320, and a negative electrode 330.

[0073] Optionally, the sodium battery 300 of this application may be, but is not limited to, at least one of sodium-ion batteries, sodium metal batteries, lithium-sodium hybrid batteries, etc.

[0074] It can be understood that the positive electrode tab 400 and the negative electrode tab 330 are located on opposite sides of the separator 320, i.e., the separator 320 is located between the positive electrode tab 400 and the negative electrode tab 330, and separates the positive electrode tab 400 and the negative electrode tab 330.

[0075] It should be noted that the positive electrode tab 400, the separator 320, and the negative electrode tab 330 are at least partially immersed in the electrolyte.

[0076] Optionally, the electrolyte includes an electrolyte salt, an organic solvent, and a film-forming additive.

[0077] Optionally, the electrolyte salt can include, but is not limited to, a sodium salt. Optionally, the sodium salt can be, but is not limited to, at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium bis(oxalato)borate, sodium difluorodioxalato phosphate, sodium difluorooxalato borate, sodium difluorophosphate (NaPO2F2), sodium triflate (CF3SO3Na), and the like.

[0078] Optionally, the organic solvent can include at least one of a cyclic carbonate and a chain carbonate. Optionally, the cyclic carbonate can include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), and the like. The dielectric constant of ethylene carbonate is much larger than that of propylene carbonate, and ethylene carbonate can better promote the formation of a solid electrolyte interface film (SEI). Optionally, the chain carbonate can include, but is not limited to, at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and the like. Optionally, the organic solvent further includes at least one of ethyl acetate, propyl acetate, ethyl propionate, propyl propionate, γ-butyrolactone, 2,2-difluoroethyl acetate.

[0079] Optionally, the film-forming additive can include, but is not limited to, at least one of propargyl benzene sulfonic acid, vinylene carbonate (VC), fluoroethylene carbonate (FEC), diethyl sulfite (DTD), methylene methane disulfonate (MMDS), butyl sulfonic acid lactone (BS), 1,3-propylene sulfonic acid lactone (PST), and the like.

[0080] Optionally, the diaphragm 320 can be, but is not limited to, at least one of a polypropylene film (PP film for short), a polyethylene film (PE film for short), a ceramic diaphragm 320, a glass fiber film, etc. Optionally, the thickness of the diaphragm 320 is 10 μm to 18 μm, and specifically, the thickness of the diaphragm 320 can be, but is not limited to, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 14.5 μm, 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm, etc.

[0081] Figure 6 A sectional view of the negative pole piece 330 of an embodiment is shown in FIG. 3.

[0082] Please refer to Figure 6 Optionally, the negative pole piece 330 includes a negative pole current collector 331 and a negative pole active layer 332, and the negative pole active layer 332 is arranged on the surface of the negative pole current collector 331.

[0083] It should be noted that the negative pole active layer 332 can be arranged on one surface or multiple surfaces (greater than or equal to two surfaces) of the negative pole current collector 331. In the schematic diagram of the drawings of the present application, the negative pole active layer 332 is arranged on the opposite two surfaces of the negative pole current collector 331, which should not be understood as a limitation of the negative pole active layer 332 and the negative pole piece 330 of the embodiments of the present application.

[0084] Optionally, the negative pole current collector 331 can be, but is not limited to, at least one of a copper foil, a copper sheet, an aluminum foil, and an aluminum sheet, etc.

[0085] Optionally, the negative pole active layer 332 includes a negative pole active material, a negative pole conductive agent, a negative pole binder, and a negative pole thickening agent, etc.

[0086] Optionally, the negative pole active material can be, but is not limited to, hard carbon.

[0087] Optionally, the negative pole conductive agent can be, but is not limited to, at least one of conductive carbon black (SP for short), acetylene black, carbon nanotubes, carbon fibers, graphene, etc.

[0088] Optionally, the negative pole binder can be, but is not limited to, at least one of polyvinylidene fluoride, polyamide, polyacrylonitrile, polyacrylate, polyvinyl ether, polymethyl methacrylate, polyhexafluoropropylene, sodium carboxymethyl cellulose (CMC for short), butadiene-styrene rubber, etc.

[0089] Optionally, the negative pole thickening agent can be, but is not limited to, at least one of polyacrylamide (PAM) and polymethyl acrylate (PMA), etc.

[0090] Please refer to Figure 4 and Figure 5Optionally, the sodium battery 300 further comprises a housing 340 and an end cap assembly 350, the housing 340 and the end cap assembly 350 enclose a closed receiving cavity (not shown in the figure) for accommodating the electrolyte, the positive electrode sheet 400, the separator 320 and the negative electrode sheet 330. It can be understood that the end cap assembly 350 is electrically connected to the positive electrode sheet 400 and the negative electrode sheet 330 respectively, and the positive electrode sheet 400 and the negative electrode sheet 330 are led out to be electrically connected to external devices or other sodium batteries 300.

[0091] Figure 7 A cross-sectional view of the positive electrode sheet 400 of an embodiment is shown.

[0092] Please refer to Figure 7 Optionally, the positive electrode sheet 400 comprises a positive electrode current collector 410 and a positive electrode active layer 420, the positive electrode active layer 420 is arranged on the surface of the positive electrode current collector 410, and the positive electrode active layer 420 comprises positive electrode particles 500.

[0093] It should be noted that the positive electrode active layer 420 can be arranged on one surface or more surfaces (greater than or equal to two surfaces) of the positive electrode current collector 410. In the schematic diagram of the drawings of the present application, the positive electrode active layer 420 is arranged on the opposite two surfaces of the positive electrode current collector 410 as an example, which should not be understood as a limitation of the positive electrode active layer 420 and the positive electrode sheet 400 of the embodiments of the present application.

[0094] It can be understood that the positive electrode particles 500 are the positive electrode active layer 420 material of the positive electrode active layer 420.

[0095] Optionally, the positive electrode current collector 410 can be, but is not limited to, an aluminum sheet, an aluminum foil and the like.

[0096] Optionally, the positive electrode active layer 420 further comprises a positive electrode conductive agent and a positive electrode binder.

[0097] Optionally, the positive electrode conductive agent can be, but is not limited to, at least one of conductive carbon black (SP for short), acetylene black, carbon nanotubes, carbon fibers, graphene and the like.

[0098] Optionally, the positive electrode binder can be, but is not limited to, at least one of polyvinylidene fluoride (PVDF), polyamide (PA), polyacrylonitrile (PAN), polyacrylate, polyvinyl ether, polymethyl methacrylate (PMMA), polyhexafluoropropylene, polymerized styrene butadiene rubber (SBR), and the like.

[0099] Figure 8 Structure diagram of the positive electrode particle 500 according to an embodiment of the present application.

[0100] Please refer to Figure 8 The positive electrode particle 500 according to an embodiment of the present application has a first porosity P1 within a range of 1 / 2 radius on the maximum cross section of the positive electrode particle 500 (e.g., a range within the dotted line O in FIG. 1A). Figure 8 The positive electrode particle 500 according to an embodiment of the present application has a second porosity P2 between 1 / 2 radius and 3 / 4 radius on the maximum cross section of the positive electrode particle 500 (e.g., a range between the dotted line O and the dotted line P in FIG. 1A). Figure 8 The positive electrode particle 500 according to an embodiment of the present application has a third porosity P3 between 3 / 4 radius and a surface of the positive electrode particle 500 (e.g., a range between the dotted line P and the dotted line Q in FIG. 1A). Figure 8 The positive electrode particle 500 according to an embodiment of the present application has a third porosity P3 between 3 / 4 radius and a surface of the positive electrode particle 500 (e.g., a range between the dotted line P and the dotted line Q in FIG. 1A).

[0101] In the embodiments of the present application, when a numerical range a to b is mentioned, it is understood that the numerical range can be any numerical value between a and b, including the end point value a and the end point value b, unless otherwise specified.

[0102] It can be understood that the porosity of the positive electrode particle 500 increases in a gradient manner from inside to outside.

[0103] Optionally, the positive electrode particle 500 includes a plurality of pores 510. The term "plurality" means greater than or equal to two, for example, can be, but is not limited to, 2, 5, 10, 30, 50, 100, 200, and the like.

[0104] It should be noted that the "maximum length direction" refers to the direction of the line between the two points farthest apart from each other in the positive electrode particle 500.

[0105] It should be noted that the first porosity P1 refers to the average porosity within 1 / 2 radius of the maximum cross-section of the positive electrode particle 500, that is, the average porosity from the center to 1 / 2 radius of the maximum cross-section of the positive electrode particle 500.

[0106] It should be noted that the second porosity P2 refers to the average porosity between 1 / 2 and 3 / 4 of the radius on the maximum cross-section of the positive electrode particle 500.

[0107] It should be noted that the third porosity P3 refers to the average porosity between 3 / 4 radius of the maximum cross-section of the positive electrode particle 500 and the surface of the positive electrode particle 500.

[0108] Understandably, the positive electrode particle 500 can be divided into inner layers from the inside out. Figure 8 The part within the dashed line O), the intermediate layer ( Figure 8 The portion between the middle dashed line O and the dashed line P) and the outer layer ( Figure 8 (The portion between the dashed lines P and Q). The porosity of the inner layer is less than that of the middle layer, and the porosity of the middle layer is less than that of the outer layer. It should be noted that the positive electrode particles 500 do not have clear boundaries; the inner, middle, and outer layers are merely artificial divisions for descriptive convenience.

[0109] The positive electrode particle 500 has a first porosity P1 in a 1 / 2 radius range of a maximum cross section of the positive electrode particle 500, a second porosity P2 between the 1 / 2 radius and a 3 / 4 radius of the maximum cross section of the positive electrode particle 500, and a third porosity P3 between the 3 / 4 radius and a surface of the positive electrode particle 500, where P1 < P2 < P3. The maximum cross section of the positive electrode particle 500 refers to a cross section in a maximum length direction of the positive electrode particle 500. By making the porosity 510 of the positive electrode particle 500 gradually increase from the inside to the outside, the positive electrode particle 500 as a whole has a lower porosity, and the positive electrode particle 500 has a higher compaction density, so that the sodium battery 300 has a higher energy density. In addition, the porosity 510 gradually increases from the inside to the outside, the surface of the positive electrode particle 500 has more porosities 510, a larger specific surface area, and a larger roughness, which is beneficial to the infiltration of the electrolyte on the surface of the positive electrode particle 500 and improves the electrolyte wettability of the positive electrode particle 500. Furthermore, the structure of the porosity 510 with a gradually decreasing porosity from the outside to the inside makes the electrolyte gradually penetrate into the inside of the positive electrode particle 500 under capillary action after the electrolyte is infiltrated on the surface of the positive electrode particle 500, so that the part with a lower porosity in the inside of the positive electrode particle 500 can also be well infiltrated by the electrolyte and has good electrolyte wettability, thereby better improving the kinetic performance of the sodium battery 300 and the rate performance of the sodium battery 300. In summary, by designing the distribution of the porosity of the positive electrode particle 500 to gradually increase from the inside to the outside, the positive electrode particle 500 has a higher powder compaction density, and the sodium battery 300 has a higher energy density while having higher kinetic performance and rate performance.

[0110] In some embodiments, the porosity of the positive electrode particle 500 gradually increases from the inside to the outside along the radial direction.

[0111] It can be understood that the porosity of the positive electrode particle 500 is the lowest at a position close to the center and the highest at a position close to the surface.

[0112] The embodiment can make the overall positive electrode particles 500 have a lower porosity, make the positive electrode particles 500 have a higher compaction density, and thus make the sodium battery 300 have a higher energy density, by making the porosity 510 of the positive electrode particles 500 gradually increase from the inside to the outside. In addition, the porosity 510 gradually increases from the inside to the outside, the surface of the positive electrode particles 500 has more porosities 510, a larger specific surface area, and a larger roughness, which is beneficial to the infiltration of the electrolyte on the surface of the positive electrode particles 500 and improves the electrolyte wettability of the positive electrode particles 500. Furthermore, the structure of the porosity 510 gradually decreases from the outside to the inside, so that after the electrolyte infiltrates on the surface of the positive electrode particles 500, the electrolyte can gradually penetrate into the inside of the positive electrode particles 500 under capillary action, so that the part with a lower porosity in the inside of the positive electrode particles 500 can also be well infiltrated by the electrolyte and has good electrolyte wettability, thereby better improving the kinetic performance of the sodium battery 300 and improving the rate performance of the sodium battery 300. In summary, the embodiment makes the positive electrode particles 500 have a higher powder compaction density by designing the gradually increasing porosity from the inside to the outside, so that the sodium battery 300 has a higher energy density and also has higher kinetic performance and rate performance.

[0113] In some embodiments, the average porosity P of the maximum cross section of the positive electrode particles 500 ranges from 5% to 30%.

[0114] Specifically, the average porosity P of the maximum cross section of the positive electrode particles 500 can be, but is not limited to, 5%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, etc.

[0115] In the embodiment, if the average porosity P of the maximum cross section of the positive electrode particles 500 is too small, the overall electrolyte wettability of the positive electrode particles 500 is reduced, and the kinetic performance and rate performance of the sodium battery 300 are reduced. If the average porosity P of the maximum cross section of the positive electrode particles 500 is too large, the powder compaction density of the positive electrode particles 500 is reduced, and the energy density of the sodium battery 300 is reduced.

[0116] Further, in some embodiments, the average porosity P of the maximum cross section of the positive electrode particles 500 ranges from 7% to 15%. This can make the positive electrode particles 500 have better electrolyte wettability, the sodium battery 300 have higher kinetic performance and rate performance, and the positive electrode particles 500 have a higher powder compaction density, and the sodium battery 300 have a higher energy density.

[0117] In some embodiments, the first porosity P1 ranges from 3% to 15%.

[0118] Specifically, the first porosity P1 can be, but is not limited to, 3%, 5%, 7%, 9%, 11%, 13%, 15%, etc.

[0119] In the present embodiment, if the first porosity P1 is too small, the electrolyte impregnation of the inner layer part of the positive electrode particle 500 is reduced, and the kinetic performance and rate performance of the sodium battery 300 are reduced; if the first porosity P1 is too large, the powder compaction density of the positive electrode particle 500 is reduced, and the energy density of the sodium battery 300 is reduced.

[0120] Further, in some embodiments, the first porosity P1 ranges from 5%≤P1≤10%. In this way, the positive electrode particle 500 has better electrolyte impregnation, the sodium battery 300 has higher kinetic performance and rate performance, and the positive electrode particle 500 has higher powder compaction density, and the sodium battery 300 has higher energy density.

[0121] In some embodiments, the second porosity P2 ranges from 7%≤P2≤18%.

[0122] Specifically, the second porosity P2 can be, but is not limited to, 7%, 8%, 10%, 12%, 14%, 16%, 18%, etc.

[0123] In the present embodiment, if the second porosity P2 is too small, the electrolyte impregnation of the inner layer and the intermediate layer part of the positive electrode particle 500 is reduced, and the kinetic performance and rate performance of the sodium battery 300 are reduced; if the second porosity P2 is too large, the powder compaction density of the positive electrode particle 500 is reduced, and the energy density of the sodium battery 300 is reduced.

[0124] Further, in some embodiments, the second porosity P2 ranges from 8%≤P2≤15%. In this way, the positive electrode particle 500 has better electrolyte impregnation, the sodium battery 300 has higher kinetic performance and rate performance, and the positive electrode particle 500 has higher powder compaction density, and the sodium battery 300 has higher energy density.

[0125] In some embodiments, the third porosity P3 ranges from 10%≤P3≤28%.

[0126] Specifically, the third porosity P3 can be, but is not limited to, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, etc.

[0127] In the present embodiment, if the third porosity P3 is too small, the electrolyte wettability of the positive electrode particle 500 as a whole is reduced, and the kinetic performance and rate performance of the sodium battery 300 are reduced; if the third porosity P3 is too large, the powder compaction density of the positive electrode particle 500 is reduced, and the energy density of the sodium battery 300 is reduced.

[0128] Further, in some embodiments, the third porosity P3 ranges from 12%≤P3≤20%. In this way, the positive electrode particle 500 has better electrolyte wettability, the sodium battery 300 has higher kinetic performance and rate performance, and the positive electrode particle 500 has higher powder compaction density, and the sodium battery 300 has higher energy density.

[0129] In some embodiments, the average porosity P of the maximum cross section of the positive electrode particle 500 ranges from 7%≤P1≤15%, the first porosity P1 ranges from 5%≤P1≤10%, the second porosity P2 ranges from 7%≤P2≤18%, and the third porosity P3 ranges from 10%≤P3≤28%. In this way, the positive electrode particle 500 has better electrolyte wettability, the sodium battery 300 has higher kinetic performance and rate performance, and the positive electrode particle 500 has higher powder compaction density, and the sodium battery 300 has higher energy density.

[0130] In some embodiments, the maximum cross section of the positive electrode particle 500 satisfies at least one of the following relationships:

[0131] (5P2+7P3) / P1>12; and

[0132] (4P1+5P2) / P3<9.

[0133] Specifically, (5P2+7P3) / P1may be, but is not limited to, 12.9, 13, 15, 17, 19, 21, 23, 25, 27, 29, 30, etc. If (5P2+7P3) / P1is too small, the porosity of the outer layer is lower than that of the inner layer (i.e., P3

[0134] Specifically, (4P1+5P2) / P3<9may be, but is not limited to, 8.9, 8, 7, 6, 5, 4, 3, 2, 1, etc. If (4P1+5P2) / P3<9is too large, the porosity of the middle layer of the positive electrode particle 500 is higher than that of the outer layer (i.e., P2>P3), the electrolyte wettability of the positive electrode particle 500 is reduced, and the kinetic performance of the sodium battery 300 is reduced; in addition, the powder compaction density of the positive electrode particle 500 is reduced, and the compaction density of the positive electrode plate 400 is reduced.

[0135] In some embodiments, the volume median particle size Dv501 of the positive electrode particles 500 ranges from 5 μm ≤ Dv501 ≤ 15 μm.

[0136] "Dv501" refers to the particle size corresponding to the cumulative particle size volume distribution percentage of 50% of the positive electrode particles 500; in other words, in the particle sample, 50% of the particle volume is composed of particles smaller than the particle size, and the other 50% of the particle volume is composed of particles larger than the particle size.

[0137] Specifically, the volume median particle size Dv501 of the positive electrode particles 500 can be, but is not limited to, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, etc.

[0138] If the volume median particle size Dv501 of the positive electrode particles 500 is too small, when the positive electrode particles 500 are made into a positive electrode slurry, the viscosity of the positive electrode slurry is too high, which makes the slurry coating uneven or even unable to be coated; the processing performance of the positive electrode slurry is reduced, and the rate performance of the positive electrode particles 500 is affected. If the volume median particle size Dv501 of the positive electrode particles 500 is too large, when the positive electrode particles 500 are coated on the positive electrode current collector 410, the positive electrode particles 500 are not well stacked on the positive electrode current collector 410, and the positive electrode current collector 410 generates excessive pressure during the rolling process of the positive electrode sheet 400, which reduces the ion conductivity of the positive electrode sheet 400, reduces the discharge capacity of the prepared sodium battery 300 under a large current, and reduces the kinetic performance of the sodium battery 300.

[0139] Further, in some embodiments, the volume median particle size Dv501 of the positive electrode particles 500 ranges from 9 μm ≤ Dv501 ≤ 9 μm. In this way, the positive electrode particles 500 have good processing performance and high kinetic performance.

[0140] In some embodiments, the particle size distribution of the positive electrode particles 500 satisfies: 1 ≤ (Dv901-Dv101) / Dv501 ≤ 4.

[0141] Specifically, (Dv901-Dv101) / Dv501 can be, but is not limited to, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, etc.

[0142] In the embodiment, if (Dv901-Dv101) / Dv501 is too small, the particle size distribution of the positive electrode particles 500 is too narrow, and the compaction density of the positive electrode particles 500 is reduced; if (Dv901-Dv101) / Dv501 is too large, Dv901 is too large, or Dv101 and Dv501 are too small, and the processing performance of the positive electrode particles 500 in the process of preparing the positive electrode slurry is reduced.

[0143] In some embodiments, the specific surface area S of the positive electrode particles 500 ranges from 5 m 2 / g≤S≤15 m 2 / g.

[0144] Specifically, the specific surface area S of the positive electrode particles 500 can be, but is not limited to, 5 m 2 / g, 6 m 2 / g, 7 m 2 / g, 8 m 2 / g, 9 m 2 / g, 10 m 2 / g, 11 m 2 / g, 12 m 2 / g, 13 m 2 / g, 14 m 2 / g, 15 m 2 / g, etc.

[0145] In the embodiment, if the specific surface area of the positive electrode particles 500 is too small, the porosity of the positive electrode particles 500 is too small, which is not conducive to the infiltration of the electrolyte, and the rate performance of the sodium battery 300 is reduced. If the specific surface area of the positive electrode particles 500 is too large, the positive electrode particles 500 have too many pores 510, and under the same formulation conditions, the flowability of the positive electrode slurry will be poor, the processing of the positive electrode sheet 400 will be poor, and the film surface will be uneven and prone to material falling, etc. In addition, the number of side reaction sites is increased, and the cycle performance of the sodium battery 300 is reduced, but the rate performance of the sodium battery 300 is improved.

[0146] Further, in some embodiments, the specific surface area S of the positive electrode particles 500 ranges from 6 m 2 / g≤S≤9 m 2 / g. In this way, the positive electrode particles 500 have high kinetic performance and cycle performance, and have good processing performance.

[0147] In some embodiments, the positive electrode particles 500 are sodium iron pyrophosphate secondary particles, and the sodium iron pyrophosphate secondary particles are composed of a plurality of sodium iron pyrophosphate primary particles; the chemical formula of the sodium iron pyrophosphate is: Na x Fe y Me z (PO4) α(P2O7) β wherein Me is at least one of Mg, Ca, Al, Ti, V, Mn, Cr, Cu, Zn, Zr, Nb, W, Mo, Sc, Y, 3.7≤x≤4.3, 2.8≤y+z≤3.0, 0≤z≤1.0, 3.9≤α+2β≤4.1.

[0148] It can be understood that the secondary particles of sodium iron pyrophosphate phosphate are formed by aggregation of a plurality of primary particles of sodium iron pyrophosphate phosphate. The number of primary particles of sodium iron pyrophosphate phosphate in the secondary particles of sodium iron pyrophosphate phosphate can be, but is not limited to, 2, 5, 10, 20, 30, 50, 80, 100, 130, 150, etc.

[0149] Specifically, x can be, but is not limited to, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, etc. If x is too small, the content of sodium element in sodium iron pyrophosphate phosphate is too small, which increases the proportion of sodium iron pyrophosphate impurities in sodium iron pyrophosphate phosphate, and reduces the gram capacity of sodium iron pyrophosphate phosphate. If x is too large, the content of sodium element in sodium iron pyrophosphate phosphate is too large, which increases the proportion of sodium iron impurities in sodium iron pyrophosphate phosphate, and reduces the gram capacity of sodium iron pyrophosphate phosphate.

[0150] Specifically, y+z can be, but is not limited to, 2.8, 2.9, 3.0, etc. If y+z is too small, the proportion of sodium iron pyrophosphate impurities in sodium iron pyrophosphate phosphate is increased, and the gram capacity of sodium iron pyrophosphate phosphate is reduced. If y+z is too large, the proportion of sodium iron impurities in sodium iron pyrophosphate phosphate is increased, and the gram capacity of sodium iron pyrophosphate phosphate is reduced.

[0151] Specifically, z can be, but is not limited to, 0, 0.1, 0.2, 0.4, 0.6, 0.8, 1.00, etc. If z is too small, the improvement effect of Me metal element on the kinetic performance of the positive electrode particles 500 is not obvious; if z is too large, the stability of the structure of sodium iron pyrophosphate phosphate is affected.

[0152] Specifically, α+2β can be, but is not limited to, 3.9, 4.0, 4.1, etc. If α+2β is too small, the proportion of sodium iron impurities in sodium iron pyrophosphate phosphate is increased, and the gram capacity of sodium iron pyrophosphate phosphate is reduced; if α+2β is too large, the proportion of sodium iron pyrophosphate impurities in sodium iron pyrophosphate phosphate is increased, and the gram capacity of sodium iron pyrophosphate phosphate is reduced.

[0153] In the present embodiment, at least one metal element selected from Mg, Ca, Al, Ti, V, Mn, Cr, Cu, Zn, Zr, Nb, W, Mo, Sc, and Y is used to modify the sodium iron phosphate pyrophosphate, so that the positive electrode particles 500 have a higher sodium ion migration rate, and the kinetic performance of the positive electrode particles 500 is improved. In addition, by designing the proportion of each element in the sodium iron phosphate pyrophosphate, the positive electrode particles 500 have a lower content of impurities and a higher specific capacity.

[0154] Figure 9 The structure of the positive electrode particles 500 according to another embodiment of the present application is shown in the schematic diagram.

[0155] Please refer to Figure 9 In some embodiments, the positive electrode particles 500 are sodium iron phosphate pyrophosphate secondary particles, which are composed of a plurality of sodium iron phosphate pyrophosphate primary particles 520; the sodium iron phosphate pyrophosphate primary particles 520 include an active core 521 and a carbon layer 522, the active core 521 is sodium iron phosphate pyrophosphate, and the carbon layer 522 is wrapped on the surface of the active core 521, and the mass fraction of the carbon layer 522 in the positive electrode particles 500 ranges from 1.0wt% to 3.0wt%.

[0156] Specifically, the mass fraction of the carbon layer 522 in the positive electrode particles 500 can be, but is not limited to, 1.0wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3.0wt%, etc.

[0157] If the mass fraction of the carbon layer 522 in the positive electrode particles 500 is too low, the electronic transmission rate of the positive electrode particles 500 is reduced, the powder resistivity of the positive electrode particles 500 is increased, and the kinetic performance of the positive electrode particles 500 is reduced. If the mass fraction of the carbon layer 522 in the positive electrode particles 500 is too high, the content of the carbon layer 522 is too high, and the specific capacity, the powder compaction density, and the compaction density of the electrode sheet of the positive electrode particles 500 are reduced.

[0158] In some embodiments, the powder compaction density of the positive electrode particles 500 is ≥2.15g / cm 3 .

[0159] Specifically, the powder compaction density of the positive electrode particles 500 can be, but is not limited to, 2.15g / cm 3 , 2.18g / cm 3 , 2.20g / cm 3 , 2.22g / cm 3 , 2.24g / cm 32.26 g / cm3 3 2.28 g / cm3 3 2.30 g / cm3 3 2.32 g / cm3 3 2.34 g / cm3 3 2.36 g / cm3 3 and so on.

[0160] In the embodiment, the powder compaction density of the positive electrode particle 500 is determined by the mass fraction and porosity of the carbon layer 522 of the positive electrode particle 500. If the powder compaction density of the positive electrode particle 500 is too low, it means that the mass fraction and porosity of the carbon layer 522 of the positive electrode particle 500 are too high, which will result in that the compaction density of the positive active layer 420 of the positive electrode sheet 400 is too low, and the energy density of the sodium battery 300 is too low. If the powder compaction density of the positive electrode particle 500 is too high, it means that the carbon content and porosity of the positive electrode particle 500 are too low, which will reduce the wettability of the electrolyte to the positive active layer 420, is not conducive to shortening the solid-phase transmission distance, reduces the play of the gram capacity of the sodium battery 300, and reduces the rate performance and low-temperature performance of the sodium battery 300.

[0161] The test method of the powder compaction density of the positive electrode particle 500 is as follows: 2g to 3g of Na4Fe3(PO4)2(P2O7) powder is added to a mold of a powder resistance instrument with a diameter of 13mm, and after being pressed to 3T, the volume and mass are measured, and the powder compaction density of the positive electrode particle 500 is calculated.

[0162] The positive electrode particle 500 of the embodiment can be prepared by the method described in the following embodiments of the application, in addition, it can also be prepared by other methods, the preparation method of the embodiment of the application is only one or more preparation methods of the positive electrode particle 500 of the application, and should not be understood as the limitation of the positive electrode particle 500 provided by the embodiment of the application.

[0163] Figure 10 The flowchart of the preparation method of the positive electrode particle 500 of the embodiment of the application is shown.

[0164] Please refer to Figure 10 The embodiment of the application provides a preparation method of a positive electrode particle 500, and the preparation method comprises the following steps:

[0165] S601, providing a sodium source, a phosphorus source, an iron source and a carbon source;

[0166] It can be understood that the raw material components of the positive electrode particle 500 include a sodium source, a phosphorus source, an iron source and a carbon source.

[0167] Optionally, the sodium source can include, but is not limited to, at least one of sodium dihydrogen phosphate, sodium pyrophosphate, sodium carbonate, sodium acetate, and these compounds containing crystal water.

[0168] Optionally, the phosphorus source can include, but is not limited to, at least one of sodium dihydrogen phosphate, sodium pyrophosphate, ammonium dihydrogen phosphate, and these compounds containing crystal water.

[0169] Optionally, the iron source can include, but is not limited to, at least one of ferrous oxalate, ferric nitrate, ferrous sulfate, and these compounds containing crystal water. For example, ferrous oxalate dihydrate.

[0170] Optionally, the carbon source is at least one of glucose, sucrose, starch, polyethylene glycol, ascorbic acid, citric acid, and the like.

[0171] S602, placing the sodium source, the phosphorus source, the iron source, and the carbon source in a solvent for sanding to obtain a slurry;

[0172] S603, spray drying the slurry to obtain a precursor powder; and

[0173] S604, sequentially pre-sintering and sintering the precursor powder to obtain the positive electrode particles 500, wherein the positive electrode particles 500 have a first porosity P1 within a 1 / 2 radius range on a maximum cross section of the positive electrode particles 500, have a second porosity P2 between the 1 / 2 radius and the 3 / 4 radius on the maximum cross section of the positive electrode particles 500, and have a third porosity P3 between the 3 / 4 radius and the surface of the positive electrode particles 500 on the maximum cross section of the positive electrode particles 500, wherein P1 < P2 < P3, and the maximum cross section of the positive electrode particles 500 refers to a cross section in a maximum length direction of the positive electrode particles 500.

[0174] The preparation method of the positive electrode particle 500 in the embodiment of the present application first pre-sinters the precursor powder and then sinters it, so that the water (including free water and bound water) in the precursor powder can be better removed during pre-sintering, thereby avoiding the increase of the content of impurities in the prepared positive electrode particle 500 and improving the tap density of the positive electrode particle 500. In addition, the positive electrode particle 500 has a first porosity P1 within a 1 / 2 radius range of a maximum cross section of the positive electrode particle 500, a second porosity P2 between the 1 / 2 radius and a 3 / 4 radius of the maximum cross section of the positive electrode particle 500, and a third porosity P3 between the 3 / 4 radius and a surface of the positive electrode particle 500, wherein P1 < P2 < P3. The maximum cross section of the positive electrode particle 500 refers to a cross section in the maximum length direction of the positive electrode particle 500. In the present application, the porosity 510 of the positive electrode particle 500 is distributed in a gradient increasing manner from the inside to the outside, so that the positive electrode particle 500 as a whole has a lower porosity and a higher tap density, thereby enabling the sodium battery 300 to have a higher energy density. In addition, the porosity 510 is distributed in a gradient increasing manner from the inside to the outside, the surface of the positive electrode particle 500 has more porosities 510, a larger specific surface area, and a larger roughness, which is beneficial to the infiltration of the electrolyte on the surface of the positive electrode particle 500 and improves the electrolyte wettability of the positive electrode particle 500. Furthermore, the structure of the porosity 510 with a gradient decreasing porosity from the outside to the inside enables the electrolyte to gradually penetrate into the inside of the positive electrode particle 500 under capillary action after the electrolyte is infiltrated on the surface of the positive electrode particle 500, so that the part with a lower porosity in the inside of the positive electrode particle 500 can also be well infiltrated by the electrolyte and has good electrolyte wettability, thereby better improving the kinetic performance of the sodium battery 300 and the rate performance of the sodium battery 300. In summary, the present application enables the positive electrode particle 500 to have a higher tap density and the sodium battery 300 to have higher energy density, kinetic performance and rate performance by designing the gradient increasing distribution of the porosity of the positive electrode particle 500 from the inside to the outside.

[0175] In some embodiments, in S602, the sodium source, the phosphorus source, the iron source and the carbon source are subjected to sand milling in the solvent to obtain a slurry, which includes: mixing the sodium source, the phosphorus source, the iron source and the carbon source in water and performing sand milling treatment to obtain the slurry, wherein the sand milling treatment time is 5h to 15h, and the sand milling speed is 100rpm to 400rpm.

[0176] It can be understood that the solvent can be, but is not limited to, water.

[0177] In the present embodiment, before spray drying, the raw materials (i.e., sodium source, phosphorus source, iron source, and carbon source) are first mixed by sand milling. Sand milling can reduce the particle size of the raw materials, providing a prerequisite for the formation of sodium iron phosphate pyrophosphate; in addition, sand milling can fully mix the soluble and insoluble substances in the raw materials, avoiding uneven mixing of the raw materials when multiple insoluble raw materials are present, which increases the probability of producing heterogeneous phases in the final formed sodium iron phosphate pyrophosphate.

[0178] Specifically, the sand milling time can be, but is not limited to, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, etc. If the sand milling time is too short, the particle size of the insoluble raw materials in the sodium source, phosphorus source, iron source, and carbon source will be too large, thereby causing local overgrowth of crystals during the subsequent sintering process, which reduces the sphericity of the prepared positive electrode particles 500; if the sand milling time is too long, the production efficiency is reduced.

[0179] Specifically, the rotation speed of sand milling can be, but is not limited to, 100rpm, 150rpm, 200rpm, 250rpm, 300rpm, 350rpm, 400rpm, etc. If the rotation speed of sand milling is too low, the particle size of the insoluble raw materials in the sodium source, phosphorus source, iron source, and carbon source will be too large, thereby causing local overgrowth of crystals during the subsequent sintering process, which reduces the sphericity of the prepared positive electrode particles 500; if the rotation speed of sand milling is too high, the slurry is easily splashed.

[0180] In some embodiments, the solid content of the slurry ranges from 20% to 50%. Specifically, the solid content of the slurry can be, but is not limited to, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, etc. In the present embodiment, if the solid content of the slurry is too low, the material cannot quickly and effectively shrink into a spherical morphology during the spray drying stage, which affects the sphericity of the final prepared positive electrode particles 500; if the solid content of the slurry is too high, it will cause great difficulty for sand milling, in addition, the material forms a ball too quickly during the spray drying stage, and there is not enough time to form a ball with high sphericity, thereby reducing the sphericity of the obtained precursor powder, and further reducing the sphericity of the final prepared positive electrode particles 500.

[0181] In some embodiments, the slurry includes solid particles, and the volume median particle size Dv50 of the solid particles ranges from 100nm≤Dv50≤300nm.

[0182] "Dv50" refers to the particle size corresponding to the cumulative particle size volume distribution percentage of 50% of the solid particles; in other words, in the particle sample, 50% of the particle volume is composed of particles smaller than the particle size, and the other 50% of the particle volume is composed of particles larger than the particle size.

[0183] Specifically, the volume median particle size Dv50 of the solid particles can be, but is not limited to, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, etc.

[0184] In this embodiment, the particle size of the solid particles in the slurry after sanding is controlled to a smaller value, so that the precursor powder can form larger primary particles through the fusion reaction of solid particles during sintering, so that the prepared positive electrode particles 500 have lower porosity. However, if the volume median particle size Dv50 of the solid particles is too small, the porosity of the prepared positive electrode particles 500 is too low, the electrolyte wettability of the positive electrode particles 500 is reduced, and the kinetic performance of the positive electrode particles 500 is reduced. In addition, if the volume median particle size of the solid particles is too small, longer sanding time is required, which increases the preparation cost of the positive electrode particles 500. If the volume median particle size Dv50 of the solid particles is too large, the raw materials are easily mixed unevenly, the proportion of impurities in the prepared positive electrode particles 500 is too high, which reduces the specific capacity of the positive electrode particles 500, and in addition, it is not conducive to the fusion growth of the positive electrode particles 500 in the subsequent sintering stage. Large pores are prone to occur, which makes the porosity too large. In addition, if the volume median particle size Dv50 of the solid particles is too small or too large, the porosity gradient distribution of the prepared positive electrode particles 500 from the inside to the outside will be affected, and it is difficult to balance the high powder compaction density and kinetic performance.

[0185] In some embodiments, in S603, the slurry is spray dried to obtain a precursor powder, including: spray drying the slurry at an inlet air temperature of 180℃≤T1≤250℃ and an outlet air temperature of 80℃≤T2≤120℃ to obtain a precursor powder.

[0186] Specifically, the inlet air temperature of the spray drying can be, but is not limited to, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃, 250℃, etc.

[0187] In the present embodiment, if the inlet air temperature of the spray drying of the slurry is too high, the solvent (such as water) evaporates too fast, and hollow spherical morphology or collapsed spherical morphology precursor powder is easily formed, affecting the processing performance and the compaction density of the final prepared positive electrode particles 500. If the inlet air temperature is too low, the solvent (such as water) evaporates too slowly, affecting the equipment productivity.

[0188] Specifically, the outlet air temperature of the spray drying can be, but is not limited to, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, etc. If the outlet air temperature of the spray drying is too low, the slurry is easy to stick to the cloth bag, and the yield is reduced. If the outlet air temperature of the spray drying is too high, the organic carbon source is easy to be carbonized.

[0189] Optionally, the volume median particle size Dv502 of the precursor powder ranges from 4 μm to 20 μm.

[0190] "Dv502" refers to the particle size corresponding to the cumulative particle size volume distribution percentage of 50% of the precursor powder; in other words, in the particle sample, 50% of the particle volume is composed of particles smaller than the particle size, and the other 50% of the particle volume is composed of particles larger than the particle size.

[0191] Specifically, the volume median particle size Dv502 of the precursor powder can be, but is not limited to, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc.

[0192] If the volume median particle size Dv502 of the precursor powder is too small, the Dv501 of the prepared positive electrode particles 500 is too small, and when the positive electrode particles 500 are made into a positive electrode slurry, the viscosity of the positive electrode slurry is too high, which makes the slurry coating uneven, or even unable to be coated; the processing performance of the positive electrode slurry is reduced, and the rate performance of the positive electrode particles 500 is affected. If the volume median particle size Dv502 of the precursor powder is too large, the Dv501 of the prepared positive electrode particles 500 is too large, which easily causes the positive electrode particles 500 to be coated on the positive electrode current collector 410, the positive electrode particles 500 have a poor stacking effect on the positive electrode current collector 410, and the positive electrode current collector 410 generates an excessive pressure during the rolling process of the positive electrode sheet 400, thereby reducing the ion conductivity of the positive electrode sheet 400, reducing the discharge capacity of the prepared sodium battery 300 under a large current, and reducing the kinetic performance of the sodium battery 300.

[0193] In some embodiments, the particle size distribution of the precursor powder satisfies: 1≤(Dv902-Dv102) / Dv502≤4.

[0194] Specifically, (Dv902-Dv102) / Dv502 can be, but is not limited to, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, etc.

[0195] In the present embodiment, if (Dv902-Dv102) / Dv502 is too small, the particle size distribution of the prepared positive electrode particles 500 is too narrow, and the tap density of the positive electrode particles 500 is reduced; if (Dv902-Dv102) / Dv502 is too large, Dv902 is too large, or Dv102 and Dv502 are too small, the particle size distribution of the prepared positive electrode particles 500 is too wide, and the processing performance of the positive electrode particles 500 in the process of preparing the positive electrode slurry is reduced.

[0196] See Figure 11 In some embodiments, in S604, the precursor powder is sequentially pre-sintered and sintered to obtain the positive electrode particles 500, which includes:

[0197] S6041, the precursor powder is heated to 250-400°C at a first heating rate to perform pre-sintering to obtain an intermediate; and

[0198] Optionally, the pre-sintering is performed under the protection of an inert atmosphere. Optionally, the inert atmosphere includes at least one of helium, nitrogen, and argon.

[0199] Specifically, the pre-sintering temperature can be, but is not limited to, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, and 400°C. If the pre-sintering temperature is too low, the moisture in the precursor powder cannot be completely removed in the pre-sintering stage, so that the content of impurities in the prepared positive electrode particles 500 after sintering is too high, and the gram capacity of the positive electrode particles 500 is reduced. If the pre-sintering temperature is too high, the content of impurities in the prepared positive electrode particles 500 will also increase, and the gram capacity of the positive electrode particles 500 is reduced.

[0200] Further, the pre-sintering temperature ranges from 275°C to 375°C. In this way, the content of impurities in the prepared positive electrode particles 500 is relatively low, and the gram capacity of the positive electrode particles 500 is improved.

[0201] Optionally, the first temperature increasing rate ranges from 2 ℃ / min to 10 ℃ / min. Specifically, the first temperature increasing rate can be, but is not limited to, 2 ℃ / min, 3 ℃ / min, 4 ℃ / min, 5 ℃ / min, 6 ℃ / min, 7 ℃ / min, 8 ℃ / min, 9 ℃ / min, 10 ℃ / min, etc. If the first temperature increasing rate is too slow, the porosity and specific surface area of the prepared positive electrode particles 500 are too large, which reduces the compaction density of the positive electrode particles 500. If the first temperature increasing rate is too fast, the porosity and specific surface area of the prepared positive electrode particles 500 are too small, which reduces the electrolyte wettability of the positive electrode particles 500 and reduces the kinetic performance of the positive electrode particles 500. In addition, too slow or too fast first temperature increasing rate will affect the gradient distribution of the porosity of the prepared positive electrode particles 500 from the inside to the outside, and it is difficult to balance the high powder compaction density and kinetic performance.

[0202] Further, the first temperature increasing rate ranges from 2 ℃ / min to 5 ℃ / min. In this way, the prepared positive electrode particles 500 have a higher compaction density.

[0203] Optionally, the pre-sintering time ranges from 3 h to 12 h. Specifically, the pre-sintering time can be, but is not limited to, 3 h, 4 h, 5 h, 6 h, 8 h, 10 h, 12 h, etc. If the pre-sintering time is too short, the bound water in the precursor powder cannot be removed, which affects the phase formation of the material during subsequent sintering. If the pre-sintering time is too long, the production energy consumption increases, which increases the preparation cost of the positive electrode particles 500.

[0204] S6042, the intermediate is heated to 500-650 ℃ at a second temperature increasing rate for sintering to obtain the positive electrode particles 500.

[0205] Optionally, the sintering is performed under the protection of an inert atmosphere. Optionally, the inert atmosphere includes at least one of helium, nitrogen, and argon.

[0206] Specifically, the sintering temperature can be, but is not limited to, 500 ℃, 510 ℃, 520 ℃, 530 ℃, 540 ℃, 550 ℃, 560 ℃, 570 ℃, 580 ℃, 590 ℃, 600 ℃, 610 ℃, 620 ℃, 630 ℃, 640 ℃, 650 ℃, etc. If the sintering temperature of the intermediate is too low, the carbonization degree of the carbon layer 522 in the prepared positive electrode particles 500 is too low, the powder resistivity of the positive electrode particles 500 is too high, the internal resistance of the sodium battery 300 is too large when the positive electrode particles 500 are applied to the sodium battery 300, and the cycle life of the sodium battery 300 is reduced. If the sintering temperature of the intermediate is too high, the sodium iron phosphate pyrophosphate in the positive electrode particles 500 is easily decomposed to form sodium iron phosphate and sodium iron pyrophosphate impurities, thereby reducing the specific capacity of the positive electrode particles 500.

[0207] Optionally, the first temperature rising rate is greater than the second temperature rising rate. The precursor powder mainly generates water vapor during the pre-sintering stage, and a greater first temperature rising rate during the pre-sintering stage can better exhaust and form pores; the intermediate mainly generates carbon dioxide during the sintering stage, and a smaller second temperature rising rate can enable the gas to be released from the inside to the outside, thereby realizing gradient pore forming and forming a gradient pore distribution.

[0208] Optionally, the second temperature rising rate ranges from 1 ℃ / min to 5 ℃ / min. Specifically, the second temperature rising rate can be, but is not limited to, 1 ℃ / min, 1.5 ℃ / min, 2 ℃ / min, 2.5 ℃ / min, 3 ℃ / min, 3.5 ℃ / min, 4 ℃ / min, 4.5 ℃ / min, 5 ℃ / min, etc. If the second temperature rising rate is too slow, the porosity and specific surface area of the prepared positive electrode particles 500 are too small, which reduces the electrolyte wettability of the positive electrode particles 500 and reduces the kinetic performance of the positive electrode particles 500. If the second temperature rising rate is too fast, the porosity and specific surface area of the prepared positive electrode particles 500 are too large, which reduces the compaction density of the positive electrode particles 500. In addition, too slow or too fast second temperature rising rate will affect the gradient distribution of the porosity of the prepared positive electrode particles 500 from the inside to the outside, and it is difficult to balance the high powder compaction density and kinetic performance.

[0209] Further, the second temperature rising rate ranges from 1 ℃ / min to 3 ℃ / min. In this way, the prepared positive electrode particles 500 can have high compaction density and high kinetic performance.

[0210] Optionally, the sintering time can be 6h to 24h. Specifically, the sintering time of the precursor powder can be, but is not limited to, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc. If the sintering time is too short, the carbonization degree of the carbon layer 522 of the prepared positive electrode particles 500 is too low, which increases the powder resistivity of the positive electrode particles 500; if the sintering time is too long, the probability of decomposition of sodium iron phosphate pyrophosphate increases, which increases the content of sodium iron phosphate impurities and sodium iron pyrophosphate impurities in the positive electrode particles 500, and reduces the specific capacity of the positive electrode particles 500.

[0211] The positive electrode particles 500 and the sodium battery 300 of the present application are further described below through specific examples.

[0212] Examples 1 to 13, Comparative Examples 1 to 6

[0213] The positive electrode particles 500 of each example and comparative example are prepared by the following steps:

[0214] (1) Sodium pyrophosphate (sodium source), ammonium dihydrogen phosphate (phosphorus source), ferrous oxalate dihydrate (iron source), and glucose (carbon source) were weighed according to a predetermined ratio, and were dispersed in water (solvent) to obtain a slurry by sand milling, wherein the solid content of the slurry was 35%, and the volume median particle size Dv50 of the solid particles in the slurry after sand milling in each example and the comparative example was shown in Table 1 below.

[0215] (2) The slurry was spray dried at 105°C to obtain a precursor powder.

[0216] (3) The precursor powder was placed in a sintering furnace, and was heated to a pre-sintering temperature at a first heating rate under nitrogen protection for 5h, and then was heated to a sintering temperature at a second heating rate for 12h, and then was cooled to obtain the positive electrode particles 500, wherein the first heating rate, the pre-sintering temperature, the second heating rate, and the sintering temperature in each example and the comparative example were shown in Table 1 below.

[0217] Sodium battery 300 assembly: (1) The positive electrode particles 500, polyvinylidene fluoride (binder), and conductive carbon black (conductive agent, Super P) were mixed in a mass ratio of 96:2:2, and were dispersed in nitrogen methyl pyrrolidone to prepare a positive electrode slurry, and then the positive electrode slurry was coated on the positive electrode current collector 410 and was dried to prepare the positive electrode sheet 400; (2) The positive electrode sheet 400, the negative electrode sheet 330, the separator 320, and the electrolyte were assembled into a soft pack battery, wherein the negative electrode sheet 330 was composed of a hard carbon negative electrode, a conductive agent, and a binder, the separator 320 was a polypropylene separator 320, the electrolyte was a carbonate electrolyte, the electrolyte included a mixed solvent of sodium hexafluorophosphate (sodium salt), ethylene carbonate, and dimethyl carbonate, and a fluoroethylene carbonate additive, and the molar concentration of sodium hexafluorophosphate in the electrolyte was 1 mol / L.

[0218] The positive electrode particles 500 and the soft pack battery of each example and the comparative example were tested for various performances.

[0219] (1) P, P1, P2, and P3 tests: After the positive electrode particles 500 were cut by an argon ion beam, a material cross-section photo was taken under an electron microscope, and then the porosity data in different interval ranges was obtained by selecting the region of the obtained cross-section photo by picture recognition software.

[0220] (2) Specific surface area of the positive electrode particles 500: The specific surface area of the positive electrode particles 500 was tested according to the method of determining the specific surface area of solid substances by gas adsorption BET method (GB / T 19587-2017).

[0221] (3) The powder compaction density test method of the positive electrode particles 500: The thickness of the aluminum foil and the mass of the aluminum foil cut into a 12 mm disc are measured in advance, then the thickness of the positive electrode sheet 400 prepared from the positive electrode particles 500 is measured, and the positive electrode sheet 400 is cut into a 12 mm disc and weighed, so as to calculate the mass and volume of the positive electrode particles 500 on the positive electrode sheet 400, and then calculate the compaction density of the positive electrode particles 500 on the positive electrode sheet 400.

[0222] (4) Rate performance test: The assembled soft package battery is tested by using the blue cell test system in the voltage range of 1.5V-3.5V at 1.0P charge / 1.0P discharge, 1.0P charge / 2.0P discharge, 1.0P charge / 3.0P discharge, and 0.5P charge / 4.0P discharge, and the rate performance is characterized by the ratio of 4.0P discharge capacity / 1.0P discharge capacity.

[0223] Table 1 Preparation process parameters of the positive electrode particles 500

[0224]

[0225] Table 2 Performance parameters of the positive electrode particles 500 and the sodium battery 300

[0226]

[0227]

[0228] From the test results of Examples 1 to 6, Comparative Example 1 and Comparative Example 2, it can be seen that when the Dv50 of the solid particles in the slurry is small (such as Comparative Example 1), the porosity of the prepared positive electrode particles 500 is small, the specific surface area of the positive electrode particles 500 is small, the powder compaction density of the positive electrode particles 500 is large, but the rate performance of the sodium battery 300 is low. With the increase of the Dv50 of the solid particles in the slurry, the porosity and specific surface area of the positive electrode particles 500 gradually increase, and the porosity gradually increases from the inside to the outside, the powder compaction density of the positive electrode particles 500 gradually decreases, and the rate performance of the sodium battery 300 gradually increases. When the Dv50 of the solid particles in the slurry is too large (such as Comparative Example 2), the porosity of the positive electrode particles 500 at each position is balanced, and the porosity of the positive electrode particles 500 from the inside to the outside does not have the increasing trend, the specific surface area is large, and the powder compaction density is reduced to a large extent.

[0229] As can be seen from the test results of Example 4, Example 7 to Example 10, Comparative Example 3 and Comparative Example 4, when the first temperature increase rate is slow during pre-sintering (such as Comparative Example 3), the porosity of the prepared positive electrode particles 500 is too large, and the porosity of each part of the positive electrode particles 500 is balanced, the specific surface area of the positive electrode particles 500 is large, and the rate performance of the positive electrode particles 500 is good, but the tap density of the positive electrode particles 500 is greatly reduced. With the increase of the first temperature increase rate during pre-sintering, the porosity of the prepared positive electrode particles 500 gradually decreases, and the porosity of the positive electrode particles 500 presents a gradient increasing distribution from the inside to the outside, the tap density of the positive electrode particles 500 gradually increases, and the rate performance of the sodium battery 300 gradually decreases. When the first temperature increase rate during pre-sintering is too fast (such as Comparative Example 4), the porosity of the positive electrode particles 500 is small, especially the internal porosity of the positive electrode particles 500 is too small, the porosity of the positive electrode particles 500 does not present an increasing distribution from the inside to the outside, and the rate performance of the sodium battery 300 is greatly reduced.

[0230] As can be seen from the test results of Example 8, Example 11 to Example 13, Comparative Example 5 and Comparative Example 6, when the second temperature increase rate is slow during sintering (such as Comparative Example 5), the porosity of the prepared positive electrode particles 500 is small, and the porosity of each part of the positive electrode particles 500 is balanced, the specific surface area of the positive electrode particles 500 is small, but the tap density of the positive electrode particles 500 is high, but the rate performance of the sodium battery 300 is greatly reduced. With the increase of the second temperature increase rate during sintering, the porosity of the prepared positive electrode particles 500 gradually increases, and the porosity of the positive electrode particles 500 presents a gradient increasing distribution from the inside to the outside, the tap density of the positive electrode particles 500 slightly decreases, and the rate performance of the sodium battery 300 gradually increases. When the second temperature increase rate during sintering is too fast (such as Comparative Example 6), the porosity of the positive electrode particles 500 is large, but the porosity of each position of the positive electrode particles 500 is balanced, and there is no increasing distribution from the inside to the outside, the rate performance of the sodium battery 300 is large, but the tap density of the positive electrode particles 500 is greatly reduced.

[0231] In the present application, the phrase "embodiment" or "embodiments" means that the specific features, structures or characteristics described in connection with the embodiment can be included in at least one embodiment of the present application. The appearance of the phrase in various places in the specification does not necessarily mean the same embodiment, nor is it an independent or alternative embodiment that is not mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in the present application can be combined with other embodiments. In addition, it should be understood that the features, structures or characteristics described in the embodiments of the present application can be combined with each other without contradiction, to form another embodiment that does not depart from the spirit and scope of the technical solution of the present application.

[0232] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application and are not limiting. Although the present application has been described in detail with reference to the above preferred embodiments, those skilled in the art should understand that the technical solutions of the present application can be modified or equivalently replaced without departing from the spirit and scope of the technical solutions of the present application.

Claims

1. A positive electrode particle, characterized by, The positive electrode particle has a first porosity P1 within a 1 / 2 radius range of a maximum cross section of the positive electrode particle, a second porosity P2 between the 1 / 2 radius and a 3 / 4 radius of the maximum cross section of the positive electrode particle, and a third porosity P3 between the 3 / 4 radius and a surface of the positive electrode particle, wherein P1 < P2 < P3, and the maximum cross section of the positive electrode particle refers to a cross section in a maximum length direction of the positive electrode particle.

2. The positive electrode particle according to claim 1, characterized by, The porosity of the positive electrode particle gradually increases from the inside to the outside along the radial direction on the maximum cross section of the positive electrode particle.

3. The positive electrode particle according to claim 1, characterized by, An average porosity P of the maximum cross section of the positive electrode particle ranges from 5% to 30%.

4. The positive electrode particle according to claim 1, characterized by, The positive electrode particle satisfies at least one of the following conditions: The first porosity P1 ranges from 3% to 15%; The second porosity P2 ranges from 7% to 18%; The third porosity P3 ranges from 10% to 28%.

5. The positive electrode particle according to claim 1, characterized by The maximum cross section of the positive electrode particle satisfies at least one of the following relationships: (5P2+7P3) / P1>12; and (4P1+5P2) / P3<9.

6. The positive electrode particle according to any one of claims 1 to 5, characterized by, The positive electrode particles are sodium iron pyrophosphate secondary particles, the sodium iron pyrophosphate secondary particles are composed of a plurality of sodium iron pyrophosphate primary particles; the chemical formula of the sodium iron pyrophosphate is: x Fe y Me z (PO4) α (P2O7) β , wherein Me is at least one of Mg, Ca, Al, Ti, V, Mn, Cr, Cu, Zn, Zr, Nb, W, Mo, Sc, Y, 3.7≤x≤4.3, 2.8≤y+z≤3.0, 0≤z≤1.0, 3.9≤α+2β≤4.

1.

7. The positive electrode particle according to any one of claims 1 to 5, characterized by, The positive electrode particle is a sodium ferric pyrophosphate secondary particle composed of a plurality of sodium ferric pyrophosphate primary particles; the sodium ferric pyrophosphate primary particle comprises an active inner core and a carbon layer, the active inner core is sodium ferric pyrophosphate, and the carbon layer is wrapped on the surface of the active inner core, and the mass fraction of the carbon layer in the positive electrode particle ranges from 1.0 wt% to 3.0 wt%.

8. A method for producing a positive electrode particle, characterized by, The preparation method comprises: providing a sodium source, a phosphorus source, an iron source, and a carbon source; sand grinding the sodium source, the phosphorus source, the iron source, and the carbon source in a solvent to obtain a slurry; spray drying the slurry to obtain a precursor powder; and sequentially pre-sintering and sintering the precursor powder to obtain the positive electrode particle, wherein the positive electrode particle has a first porosity P1 within a 1 / 2 radius range of a maximum cross section of the positive electrode particle, a second porosity P2 between the 1 / 2 radius and a 3 / 4 radius of the maximum cross section of the positive electrode particle, and a third porosity P3 between the 3 / 4 radius and a surface of the positive electrode particle, wherein P1 < P2 < P3, and the maximum cross section of the positive electrode particle refers to a cross section in a maximum length direction of the positive electrode particle.

9. The method for producing a positive electrode particle according to claim 8, characterized by, The slurry comprises solid particles, and a volume median particle size Dv50 of the solid particles ranges from 100 nm to 300 nm.

10. The method for producing a positive electrode particle according to claim 8 or 9, characterized by, The sequentially pre-sintering and sintering the precursor powder to obtain the positive electrode particle comprises: pre-sintering the precursor powder at a first temperature increasing rate to 250-400°C to obtain an intermediate; and sintering the intermediate at a second temperature increasing rate to 500-650°C to obtain the positive electrode particle.

11. The method for producing a positive electrode particle according to claim 10, characterized by, The first temperature increasing rate ranges from 2°C / min to 10°C / min, and the second temperature increasing rate ranges from 1°C / min to 5°C / min.

12. A positive electrode sheet characterized by comprising: The positive electrode tab comprises: a positive electrode current collector; and A positive electrode active layer comprising the positive electrode particle of any one of claims 1-7 or the positive electrode particle prepared by the method of any one of claims 8-11.

13. A sodium battery, characterized by, The sodium battery comprises an electrolyte, the positive electrode plate of claim 12, a separator, and a negative electrode plate.