Chromium-free high-temperature shift catalyst as well as preparation method and application thereof
By optimizing the active components such as Fe, Mn, Ni, and Cu, and the auxiliary agents K and Y, a chromium-free high-temperature conversion catalyst was developed, which solved the problems of easy catalyst sintering, side reactions, and insufficient sulfur resistance, thus achieving efficient CO conversion and environmentally friendly industrial applications.
Patent Information
- Application Number
- CN202510908778.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-02
- Publication Date
- 2025-11-07
AI Technical Summary
Existing high-temperature shift catalysts are prone to sintering and deactivation at high temperatures, side reactions affect product quality, have limited sulfur resistance, and contain hexavalent chromium, an environmentally toxic substance, which limits their application and promotion in industry.
Using active components such as Fe, Mn, Ni, and Cu, and auxiliary agents such as K and Y, combined with alumina as a support, a chromium-free high-temperature conversion catalyst was prepared by achieving uniform distribution of nanoscale active components and a highly stable support structure through ammonia water neutralization precipitation and crystal transformation processes.
It achieves high CO conversion rate, low by-product content and complete elimination of Cr6+, meets environmental regulations, and provides an efficient, green and widely adaptable solution for industrial hydrogen production.
Smart Images

Figure BDA0005479426340000071 
Figure BDA0005479426340000081
Abstract
Description
TECHNICAL FIELD
[0001] The present application belongs to the technical field of catalysts, and particularly relates to a chromium-free high-temperature shift catalyst, a preparation method and application thereof. BACKGROUND
[0002] The high-temperature shift (HTS) reaction of carbon monoxide (CO) is an indispensable key step in the fields of modern industrial hydrogen production, ammonia synthesis and coal chemical industry. The reaction is mainly based on the water-gas shift reaction (CO + H2O → CO2 + H2), which is carried out at high temperature (350-500℃) and utilizes catalysts to efficiently convert CO into CO2 while increasing the yield of hydrogen (H2) to meet the needs of downstream industries.
[0003] Currently, HTS catalysts are mainly divided into two categories: iron-chromium (Fe3O4-Cr2O3) and cobalt-molybdenum (Co-Mo / Al2O3). Iron-chromium catalysts are widely used in shift processes with low or no sulfur due to their high activity and long service life, while cobalt-molybdenum catalysts are suitable for high-sulfur environments such as hydrogen production from coal gasification or refinery gas treatment.
[0004] Although existing catalysts have been widely used in industrial production, there are still many technical bottlenecks that limit their further optimization and promotion.
[0005] The deficiencies of the prior art are as follows: 1) catalyst sintering deactivation: iron-chromium catalysts may undergo grain growth and sintering when operating at high temperatures (>400℃), leading to a decrease in specific surface area and a significant reduction in activity. In addition, carbon deposition exacerbates catalyst deactivation, shortens the service life of the catalyst, and affects the stability of industrial production.
[0006] 2) side reactions affecting product quality: under high-temperature conditions, HTS catalysts may induce the methanation side reaction (CO + 3H2 → CH4 + H2O), causing hydrogen loss and reducing the selectivity of the shift reaction. In addition, some catalysts may promote the formation of partial by-products, such as incomplete conversion of carbon monoxide or excessive oxidation of hydrogen, affecting the purity of downstream hydrogen.
[0007] 3) limited sulfur tolerance: iron-chromium catalysts are easily affected by sulfur poisoning in sulfur-containing gas environments, leading to a significant decrease in activity, making them difficult to apply in sulfur-containing conditions such as hydrogen production from coal gasification. While cobalt-molybdenum catalysts have some sulfur tolerance, their catalytic activity is relatively low, limiting their industrial application.
[0008] Due to increasingly stringent environmental regulations, traditional iron-chromium catalysts contain hexavalent chromium (Cr 6+ ), which has high environmental toxicity and poses a potential threat to human health. With the tightening of global environmental regulations, how to reduce Cr6+ Improving the content of chromium-free catalysts and even developing chromium-free catalysts has become an important research direction in current catalyst development. Summary of the Invention
[0009] To address the aforementioned technical problems, the present invention aims to provide a breakthrough chromium-free high-temperature shift catalyst. Through innovative optimization of active components such as Fe, Mn, Ni, and Cu, auxiliary agents such as K and Y, and alumina as a support, combined with a unique ammonia water neutralization precipitation and crystal transformation process (50–80℃, 1–8h), a uniform distribution of nanoscale active components and a highly stable support structure are achieved. This catalyst exhibits excellent CO conversion rate and low by-product content, and completely eliminates chromium... 6+ It complies with environmental regulations and provides an efficient, green, and widely adaptable solution for industrial hydrogen production.
[0010] This invention is achieved through the following technical solution:
[0011] A chromium-free high-temperature shift catalyst, the catalyst being composed of the following components in parts by mass:
[0012] The active component comprises 218.94–297.65 parts, the auxiliary agent comprises 0–13.07 parts, and the catalyst support comprises 70–80 parts;
[0013] The active metal components are Fe, Mn, Ni, and Cu;
[0014] The auxiliary metals are K and Y;
[0015] The catalyst support is alumina.
[0016] A method for preparing a chromium-free high-temperature shift catalyst includes the following steps:
[0017] S1. Select the active ingredient metal precursor and dissolve it in water to prepare solution A;
[0018] S2. Under stirring conditions, ammonia solution is introduced to neutralize and precipitate the substance;
[0019] S3. After the neutralization and precipitation reaction is completed, the temperature is raised to transform the crystal form of the ferric hydroxide precipitate, wash the precipitate, concentrate it, and then add a portion of the active ingredient metal precursor, auxiliary metal precursor and catalyst support precursor. After mixing evenly, it is dried, granulated, baked, and tableted with tableting lubricant. After calcination again, the product is obtained.
[0020] Preferably, in S1, the active metal precursor is ferrous sulfate, manganese sulfate, nickel nitrate, or copper nitrate.
[0021] The mass ratio of ferrous sulfate, manganese sulfate, nickel nitrate, and copper nitrate is:
[0022] In the S1, the mass concentration of Fe in the solution A is 100-150 g / L.
[0023] Preferably, in the S2, the mass concentration of the ammonia solution is 12-18%.
[0024] Preferably, in the S2, the pH in the neutralization and precipitation reaction is 7-8.
[0025] Preferably, in the S3, the temperature is raised to 50-80℃.
[0026] Preferably, the time for the crystal form conversion of the iron hydroxide precipitate is 1-8 h.
[0027] Preferably, the auxiliary metal precursor is potassium nitrate or yttrium nitrate.
[0028] The catalyst carrier precursor is pseudo-boehmite.
[0029] The tabletting lubricant is graphite.
[0030] The mass ratio of the potassium nitrate, yttrium nitrate, pseudo-boehmite and graphite is.
[0031] Preferably, the calcination temperature is 300-400℃, and the time is 1-1.2 h.
[0032] The application of a chromium-free high-temperature shift catalyst, which is applied in the high-temperature shift reaction of carbon monoxide.
[0033] Compared with the prior art, the present application has at least the following technical effects:
[0034] The present application provides a breakthrough chromium-free high-temperature shift catalyst, which realizes the uniform distribution of nanoscale active components and the high-stability carrier structure by innovatively optimizing Fe, Mn, Ni, Cu and other active components, K, Y and other auxiliary agents, and alumina as the carrier, and combining a unique ammonia neutralization and precipitation and crystal form conversion process (50-80℃, 1-8 h). The catalyst exhibits excellent CO conversion rate and low byproduct content, and completely eliminates Cr 6+ , meets environmental protection regulations, and provides an efficient, green and widely adaptable solution for industrial hydrogen production. DETAILED DESCRIPTION
[0035] The embodiments of the present application will be described in detail below with reference to the examples, but those skilled in the art will understand that the following examples are only for illustration of the present application and should not be regarded as limiting the scope of the present application. The specific conditions not mentioned in the examples are carried out according to the conventional conditions or the conditions recommended by the manufacturer, and the reagents or instruments not mentioned by the manufacturer are conventional products that can be purchased on the market.
[0036] Example 1
[0037] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0038] 218.94 g of ferrous sulfate (Fe(NO3)2), 24.43 g of manganese sulfate (Mn(NO3)2), and 11.51 g of (Ni(NO3)2) are dissolved in water to form solution A, and the concentration of Fe in the solution is 125 g / L;
[0039] Under stirring, 15% ammonia water solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0040] After neutralization, the temperature is increased to 70°C, the crystal form of the Fe(OH)3 precipitate is converted, the crystal form conversion time is 6 h, the precipitate is washed, and then 7.39 g of copper nitrate (Cu(NO3)2), 2.07 g of potassium nitrate (KNO3), 4.64 g of yttrium nitrate (YNO3), and 77.07 g of pseudo-boehmite are added, and the mixture is uniformly mixed, dried, granulated, dried, and then 10 g of graphite is added and pressed into a tablet, which is calcined at 400°C for 1 h to obtain catalyst A.
[0041] Example 2
[0042] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0043] 218.94 g of ferrous sulfate (Fe(NO3)2), 36.48 g of manganese sulfate (Mn(NO3)2) are dissolved in water to form solution A, and the concentration of Fe in the solution is 125 g / L.
[0044] Under stirring, 15% ammonia water solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0045] After neutralization, the temperature is increased to 70°C, the crystal form of the Fe(OH)3 precipitate is converted, the crystal form conversion time is 6 h, the precipitate is washed, and then 7.39 g of copper nitrate (Cu(NO3)2), 2.07 g of potassium nitrate (KNO3), 4.64 g of yttrium nitrate (YNO3), and 77.07 g of pseudo-boehmite are added, and the mixture is uniformly mixed, dried, granulated, dried, and then 10 g of graphite is added and pressed into a tablet, which is calcined at 400°C for 1 h to obtain catalyst B.
[0046] Example 3
[0047] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0048] 218.94 g of ferrous sulfate (Fe(NO3)2), 34.84 g of (Ni(NO3)2) are dissolved in water to form solution A, and the concentration of Fe in the solution is 125 g / L.
[0049] Under stirring, the 15% ammonia water solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0050] After the neutralization is completed, the temperature is increased to 70°C, the crystal form of the Fe(OH)3 precipitate is converted, the crystal form conversion time is 6h, the precipitate is washed, and then 7.39g of copper nitrate (Cu(NO3)2), 2.07g of potassium nitrate (KNO3), 4.64g of yttrium nitrate (YNO3) and 77.07g of pseudo-boehmite are added, the mixture is uniformly mixed, dried, granulated, dried, 10g of graphite is added, and then tableted, and then calcined at 400°C for 1h to obtain the catalyst C.
[0051] Example 4:
[0052] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0053] 218.94g of ferrous sulfate (Fe(NO3)2), 24.43g of manganese sulfate (Mn(NO3)2) and 11.51g of (Ni(NO3)2) are dissolved in water to prepare a solution A, and the concentration of Fe in the solution is 125g / L.
[0054] Under stirring, the 15% ammonia water solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0055] After the neutralization is completed, the temperature is increased to 70°C, the crystal form of the Fe(OH)3 precipitate is converted, the crystal form conversion time is 6h, the precipitate is washed, and then 7.39g of copper nitrate (Cu(NO3)2), 2.07g of potassium nitrate (KNO3), 4.64g of yttrium nitrate (YNO3) and 77.07g of pseudo-boehmite are added, the mixture is uniformly mixed, dried, granulated, dried, 10g of graphite is added, and then tableted, and then calcined at 400°C for 1h to obtain the catalyst C.
[0056] Example 5:
[0057] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0058] 218.94g of ferrous sulfate (Fe(NO3)2), 24.43g of manganese sulfate (Mn(NO3)2) and 11.51g of (Ni(NO3)2) are dissolved in water to prepare a solution A, and the concentration of Fe in the solution is 125g / L.
[0059] Under stirring, the 15% ammonia water solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0060] The temperature is raised to 70℃ at the end of neutralization, the crystal form of Fe(OH)3 precipitate is converted, the crystal form conversion time is 6h, the precipitate is washed, 7.39g copper nitrate (Cu(NO3)2), 5.95g potassium nitrate (KNO3) and 77.07g pseudo-boehmite are added after concentration, then the mixture is uniformly mixed, dried, granulated, dried, 10g graphite is added, then pressed into tablets, calcined at 400℃ for 1h, and catalyst E is obtained.
[0061] Example 6:
[0062] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0063] 218.94g ferrous sulfate (Fe(NO3)2), 36.48g manganese sulfate (Mn(NO3)2) are dissolved in water to prepare solution A, the concentration of Fe in the solution is 125g / L.
[0064] Under stirring, 15% ammonia solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0065] The temperature is raised to 70℃ at the end of neutralization, the crystal form of Fe(OH)3 precipitate is converted, the crystal form conversion time is 6h, the precipitate is washed, 7.39g copper nitrate (Cu(NO3)2), 5.95g potassium nitrate (KNO3) and 77.07g pseudo-boehmite are added after concentration, then the mixture is uniformly mixed, dried, granulated, dried, 10g graphite is added, then pressed into tablets, calcined at 400℃ for 1h, and catalyst E is obtained.
[0066] Example 7:
[0067] A preparation method of a chromium-free high-temperature shift catalyst, comprising the following steps:
[0068] 218.94g ferrous sulfate (Fe(NO3)2), 36.48g manganese sulfate (Mn(NO3)2) are dissolved in water to prepare solution A, the concentration of Fe in the solution is 125g / L.
[0069] Under stirring, 15% ammonia solution B is introduced for neutralization and precipitation, and the pH is controlled at 7-8.
[0070] The temperature is raised to 70℃ at the end of neutralization, the crystal form of Fe(OH)3 precipitate is converted, the crystal form conversion time is 6h, the precipitate is washed, 7.39g copper nitrate (Cu(NO3)2), 5.95g potassium nitrate (KNO3) and 77.07g pseudo-boehmite are added after concentration, then the mixture is uniformly mixed, dried, granulated, dried, 10g graphite is added, then pressed into tablets, calcined at 400℃ for 1h, and catalyst E is obtained.
[0071] Table 1 Catalyst physical and chemical properties
[0072]
[0073]
[0074] Catalyst activation: activation under hydrogen at 230℃ for 10h.
[0075] Catalyst evaluation: raw gas: H2O and CO; raw gas volume ratio 1-2:1, reaction temperature: 250℃, space velocity: 2000h-1, reaction pressure: 0.5MPa. The products were analyzed qualitatively and quantitatively by gas chromatography. -1
[0076] Table 2 Catalyst performance comparison table
[0077] Catalyst CO conversion, % Outlet methanol content, ppm Catalyst A 83 58 Catalyst B 78 69 Catalyst C 68 88 Catalyst D 72 79 Catalyst E 75 63 Catalyst F 79 68 Catalyst G 76 71
[0078] In summary: the catalysts (A-G) of Examples 1-7 exhibit excellent performance, with catalyst A (Fe 68%, Mn 7.5%, Ni 3.7%, Cu 2.5%, K 0.8%, Y 1.5%, Al 16%) performing best, with a CO conversion of 83% and a methanol content as low as 58ppm. The synergistic effect of Mn, Ni, Y and other additives enhances the performance of the catalyst, completely eliminating Cr 6+ , meeting strict environmental regulations.
[0079] The technical solution develops an innovative chromium-free high-temperature shift catalyst, by precisely regulating Fe (68%), Mn (7.5-11.2%), Ni (0-11.2%), Cu (2.5%), K (0-2.3%), Y (0-2.3%) and Al (16%) and other components, combined with ammonia water neutralization and precipitation (pH 7-8), crystal transformation (50-80℃, 1-8h) and high-temperature calcination (400℃, 1h) process, realizing nanoscale active component distribution and high stability carrier structure.
[0080] The catalyst has high activity, high selectivity, long service life and environmental friendliness, providing a revolutionary solution for industrial hydrogen production, ammonia synthesis and coal chemical industry, and has significant industrial application value and market competitiveness.
[0081] Finally, it should be noted that the above description is only a preferred embodiment of the present application and is not intended to limit the protection scope of the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A chromium-free high temperature shift catalyst, characterized in that, The catalyst is composed of components in the following mass fractions: The active component is 218.94-297.65 parts, the auxiliary agent is 0-13.07 parts, and the catalyst carrier is 70-80 parts; The active ingredient metal is Fe, Mn, Ni, and Cu; The auxiliary metal is K and Y; The catalyst carrier is alumina.
2. A process for preparing a chromium-free high temperature shift catalyst as claimed in claim 1, characterized in that, The method comprises the following steps: S1, selecting an active ingredient metal precursor to be dissolved in water to prepare solution A; S2, under stirring, ammonia solution is introduced for neutralization and precipitation; S3, after the neutralization and precipitation reaction is completed, the temperature is raised, the crystal form of the iron hydroxide precipitate is converted, the precipitate is washed, concentrated, and then a part of the active ingredient metal precursor, the auxiliary metal precursor, and the catalyst carrier precursor are added and mixed uniformly, dried, granulated, dried, pressed into tablets with a lubricant, and then calcined again to obtain the catalyst.
3. The method of claim 2, wherein the chromium-free high-temperature shift catalyst is prepared by the steps of: In S1, the active ingredient metal precursor is ferrous sulfate, manganese sulfate, nickel nitrate, and copper nitrate. The mass ratio of the ferrous sulfate, manganese sulfate, nickel nitrate, and copper nitrate is 1:1:1:
1. In S1, the mass concentration of Fe in solution A is 100-150 g / L.
4. The method of claim 2, wherein the chromium-free high-temperature shift catalyst is prepared by the steps of: In S2, the mass concentration of the ammonia solution is 12-18%.
5. The method of claim 2, wherein the chromium-free high-temperature shift catalyst is prepared by the steps of: In S2, the pH in the neutralization and precipitation reaction is 7-8.
6. The method of claim 2, wherein the chromium-free high-temperature shift catalyst is prepared by the steps of: In S3, the temperature is raised to 50-80℃.
7. The method for preparing a chromium-free high-temperature shift catalyst according to claim 2, characterized in that, The crystal form conversion time of the iron hydroxide precipitate is 1-8 h.
8. The method for preparing a chromium-free high-temperature shift catalyst according to claim 2, characterized in that, The auxiliary metal precursor is potassium nitrate and yttrium nitrate. The catalyst carrier precursor is pseudo-boehmite. The tablet lubricant is graphite. The mass ratio of the potassium nitrate, yttrium nitrate, pseudo-boehmite, and graphite is 1:1:1:
1.
9. The method of claim 2, wherein the chromium-free high-temperature shift catalyst is prepared by the steps of: The calcination temperature is 300-400℃, and the time is 1-1.2 h.
10. Use of a chromium-free high-temperature shift catalyst according to claim 1, characterized in that The catalyst is applied in the high-temperature carbon monoxide shift reaction.