Method for preparing geopolymer cementing material based on alkaline solution modified dolomite

By modifying dolomite in an alkaline solution to precipitate Ca2+ and Mg2+, thereby improving its activity and controlling the mass percentage of dolomite in the geopolymer precursor, the problems of long early-stage solidification time and low strength of geopolymers were solved, achieving efficient material utilization and performance improvement.

CN121021022APending Publication Date: 2025-11-28HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511137425.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-14
Publication Date
2025-11-28

AI Technical Summary

Technical Problem

Existing geopolymer admixtures are difficult to effectively control early setting time and mechanical properties, especially low-calcium geopolymers, which result in prolonged setting time and slow strength growth, limiting their widespread application.

Method used

By modifying dolomite in an alkaline solution to precipitate Ca2+ and Mg2+, its activity is improved. The mass percentage of dolomite in the geopolymer precursor is also controlled. The modified alkaline-activated solution is used to promote the reaction, shorten the setting time, and improve the strength.

Benefits of technology

It significantly shortens the setting time of geopolymers, improves their later strength, realizes the high-value utilization of low-value dolomite materials, and solves the problem of low early performance and mechanical properties of geopolymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121021022A_ABST
    Figure CN121021022A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of geopolymer materials, and particularly provides a method for preparing a geopolymer cementing material based on alkaline solution modified dolomite. The method specifically comprises the following steps: mixing an alkali-activated solution with dolomite to prepare a modified alkali-activated solution; the dolomite is mixed with a geopolymer precursor, the geopolymer cementing material is obtained, and the dolomite accounts for 5%-10% of the mass of the polymer precursor. According to the invention, precipitation of Ca < 2 + > and Mg < 2 + > or generation of Ca (OH) 2 in dolomite is promoted in an alkaline environment, the reaction activity is improved, the material strength is improved while the coagulation time is shortened, and the problems of delayed coagulation and mechanical property reduction caused by traditional direct addition of dolomite are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of geopolymer materials technology, and more specifically to a method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite. Background Technology

[0002] Geopolymers are amorphous cementitious materials formed by the activation of siliceous aluminosilicate precursors such as metakaolin, fly ash, and slag using an alkaline solution. The production process of geopolymers is energy-efficient, with CO2 emissions only about 20% of those of traditional silicate cement, and produces almost no harmful gases such as nitrogen oxides and sulfur oxides, effectively addressing the environmental problems associated with cement production. Furthermore, in addition to possessing mechanical strength comparable to traditional silicate cement, they exhibit better resistance to high temperatures and acid / alkali corrosion. Moreover, geopolymers have a wide range of raw material sources; the utilization of industrial wastes such as fly ash and slag not only reduces costs but also mitigates environmental pollution caused by industrial waste. Therefore, geopolymers are an economical and environmentally friendly cementitious material, considered one of the most promising cement alternatives currently available.

[0003] However, as a new type of cementitious material, geopolymers are not well-suited to admixtures currently widely used in silicate cement due to their high alkalinity and different reaction mechanisms. In particular, for low-calcium geopolymers represented by metakaolin or low-calcium fly ash, the control of early setting time can only rely on changing the mix proportion. However, changing the mix proportion will affect the later strength, which greatly restricts the promotion and application of geopolymers.

[0004] Dolomite is abundant and inexpensive, and its activity as a main precursor is very low. For example, in Reference 1: EA Aizat, AMM Al Bakri, YM Liew, CY Heah, MMA Abdullah, MM Ramli, et al. Chemical composition and strength of dolomite geopolymercomposites. AIP conference proceedings, 2017, 1885(1). In Reference 1, Aizat et al., when attempting to prepare geopolymers using dolomite as the main precursor, found that the maximum compressive strength of the prepared geopolymer was only 5 MPa, far below the standard required for practical applications. Summary of the Invention

[0005] To address the problem that existing geopolymer admixtures are difficult to control the early properties and mechanical properties of geopolymers, this invention provides a method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite.

[0006] This invention attempts to use dolomite as an inert filler and directly add it to geopolymers to prepare new geopolymer cementitious materials. However, due to the low activity of dolomite, the prepared geopolymer cementitious materials suffer from problems such as increased setting time, slow strength growth, and decreased strength in the later stages.

[0007] Based on this, the present invention modifies dolomite by using the alkalinity of the alkali-activated solution, which is beneficial to the Ca content in the dolomite. 2+ and Mg 2+ The precipitation of dolomite increases the active ingredients; at the same time, by controlling the mass percentage of dolomite in the geopolymer precursor, the reactivity of dolomite is improved, thereby shortening the geopolymer solidification time, improving the later strength, realizing the low-carbon utilization of dolomite, and realizing the high-value utilization of low-value dolomite materials.

[0008] To achieve the above objectives, the technical solution of the present invention is as follows.

[0009] This invention provides a method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite, comprising the following steps: The alkaline activation solution was mixed with dolomite for modification to obtain a modified alkaline activation solution; in the modified alkaline activation solution, SiO2 and Ca... 2+ Mg 2+ The molar ratio is 1.9:0.1~0.3:0.1~0.3.

[0010] The modified alkaline activation solution was mixed and stirred with the geopolymer precursor to obtain the geopolymer cementitious material; the mass percentage of dolomite in the geopolymer precursor was 5% to 10%.

[0011] This invention first utilizes the alkalinity of an alkaline activation solution to modify dolomite through mixing, thereby reducing the Ca content in the dolomite. 2+ and Mg 2+ The precipitation process increases the amount of active ingredients. At the same time, by adjusting the mass percentage of dolomite in the geopolymer precursor, the reactivity of dolomite is improved, thereby increasing the reaction rate of the geopolymer precursor. This leads to a reduction in setting time while increasing strength, thus solving the problem of low mechanical properties in existing geopolymers.

[0012] Preferably, the alkaline activation solution is a silicate solution with a modulus of 1.5 to 2. More preferably, the silicate solution has a modulus of 1.8 to 1.9.

[0013] In this invention, the degree of reduction in setting time varies depending on the modulus of the alkaline activation solution. Therefore, by adjusting the modulus of the alkaline activation solution, the setting time can be further controlled.

[0014] Preferably, the alkaline activation solution is a sodium silicate solution or a potassium silicate solution.

[0015] Preferably, the mixing time between the alkaline activation solution and dolomite is 24h to 48h. This invention regulates the mixing time between the alkaline activation solution and dolomite, thereby effectively promoting the precipitation of Ca in the dolomite. 2+ and Mg 2+ It precipitates out, increasing the amount of active ingredients.

[0016] Preferably, the pH of the modified alkaline activation solution is 13-14.

[0017] This invention modifies the pH, degree of polymerization, ion concentration, and particle composition of the modified alkaline activation solution by adding dolomite, thereby affecting the dissolution and condensation reaction rates of the precursor and ultimately controlling the setting time of the geopolymer. The geopolymer obtained using this method exhibits a significantly shortened setting time while maintaining its later performance.

[0018] Preferably, the geopolymer precursor is metakaolin or fly ash.

[0019] This invention addresses the problem of slow early-stage setting and low later-stage strength in low-calcium geopolymers by modifying dolomite through the alkalinity of an alkaline activation solution. This modified alkaline activation solution is then used to activate the low-calcium geopolymer precursor, thereby improving the dolomite's activity, shortening the geopolymer's setting time, increasing its strength, and enabling the high-value utilization of low-value dolomite materials.

[0020] Preferably, the time for mixing and stirring the modified alkaline activation solution with the geopolymer precursor is 4 min to 5 min.

[0021] The beneficial effects of this invention are: 1. This invention first utilizes the alkalinity of an alkaline activation solution to modify dolomite through mixing, thereby reducing the Ca content in the dolomite. 2+ and Mg 2+ The precipitation process increases the amount of active ingredients. At the same time, by adjusting the mass percentage of dolomite in the geopolymer precursor, the reactivity of dolomite is improved, thereby increasing the reaction rate of the geopolymer precursor. This leads to a reduction in setting time while improving the later-stage strength, thus solving the problem of low mechanical properties in existing geopolymers.

[0022] 2. This invention mainly modifies the SiO2 and Ca in the modified alkaline activation solution. 2+ and Mg 2+By adjusting the molar ratio of dolomite to the polymer precursor and controlling the mass percentage of dolomite, the time shortened by modification accounts for 54.5% to 72.7% of the total retarding time caused by directly adding unmodified dolomite, and the 28-day compressive strength is increased to 48.5 MPa to 52 MPa.

[0023] 3. The method of the present invention is simple and easy to implement, and can effectively reduce energy consumption. Attached Figure Description

[0024] Figure 1 These are the sinking depth curves of the polymer cementitious materials in Examples 3 to 4 and Comparative Examples 1 to 3 as a function of time.

[0025] Figure 2 These are the sinking depth curves of the polymer cementitious materials in Examples 1-2 and Comparative Examples 1-3 as a function of time.

[0026] Figure 3 This is a comparison chart of the compressive strength of geopolymer samples from Examples 3 to 4 and Comparative Examples 1 to 3 under different curing times.

[0027] Figure 4 This is a comparison chart of the compressive strength of geopolymer samples from Examples 1 to 2 and Comparative Examples 1 to 3 under different curing times.

[0028] Figure 5 The results show the concentration of dissolved ions in the polymer gelling materials of Examples 1, 2, and Comparative Example 3.

[0029] Figure 6 The results are for the determination of leached ion concentrations of the polymer gelling materials in Examples 3 and 4 and Comparative Example 3. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0031] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] Dolomite's main component is calcium magnesium carbonate, with the chemical formula CaMg(CO3)2. As an inert material, dolomite exhibits low reactivity as a primary precursor, making it difficult to effectively participate in the reaction of geopolymer systems. Therefore, most current research focuses on the application of dolomite as a filler material, failing to fully explore the potential of its chemical and mineral components. For example, in reference 1, Aizat et al., when attempting to prepare geopolymers using dolomite as the primary precursor, found that the maximum compressive strength of the prepared geopolymer was only 5 MPa, far below the standard required for practical applications.

[0033] This invention attempts to use dolomite as a mineral additive and add it directly to the geopolymer system. However, due to the low activity of dolomite, the prepared geopolymer cementitious material has a slow reaction rate and a long setting time, resulting in slow strength growth and reduced strength in the later stages.

[0034] Based on this, this invention proposes a milder and more energy-efficient method for preparing geopolymer cementitious materials. This invention utilizes an alkaline environment to chemically react hydroxide ions with calcium and magnesium carbonate in dolomite, generating calcium and magnesium ions, or calcium hydroxide and magnesium hydroxide. The theoretical basis of this modification method is that an alkaline environment can disrupt the crystal structure of calcium and magnesium carbonate through chemical dissolution, promoting its decomposition into highly reactive calcium and magnesium ions, thereby avoiding the high energy consumption problem of high-temperature pretreatment. The reaction of hydroxide ions in the alkaline solution with calcium and magnesium carbonate generates soluble calcium ions and calcium hydroxide. These calcium ions and calcium hydroxide can effectively regulate the Si / Al ratio of the geopolymer system, accelerate the dissolution of metakaolinite and the formation of aluminosilicate gel, thereby significantly shortening the early setting time of the geopolymer, improving its strength, and realizing the high-value utilization of low-value dolomite materials.

[0035] The method of this invention can significantly shorten the setting time even for dolomite particles with slightly larger particle sizes. Therefore, the method of this invention is applicable to the high-value utilization of dolomite particles of different sizes.

[0036] The reaction principle of modifying dolomite using an alkaline-activated solution is as follows: CaMg(CO3)2+ OH - →CaCO3 + Mg(OH)2 + CO3 2- .

[0037] The step of modifying dolomite using an alkaline activation solution is mainly used to control the pH value of the modified alkaline activation solution, the degree of polymerization of sodium silicate solution, the ion concentration, and the particle composition of the reaction product. In this step, sodium silicate solution reacts with dolomite to generate active calcium and magnesium ions, which are then mixed with metakaolin to prepare a geopolymer gel material. The calcium and magnesium ions accelerate the reaction process of the geopolymer, thereby affecting the degree of polymerization of sodium silicate solution.

[0038] Regarding the determination of the amount of raw materials, this invention mainly uses the molar ratio of Na2O, Al2O3, SiO2, and H2O of 1:1:4:12 as the basic ratio of geopolymer gel material, and then uses the mass percentage of dolomite as geopolymer precursor of 5% to 10% to finally determine the ratio of raw materials.

[0039] Using a molar ratio of Na₂O, Al₂O₃, SiO₂, and H₂O of 1:1:4:12 as the basic formulation for geopolymer gel materials ensures the full dissolution of aluminosilicate precursors, such as metakaolin, in an alkaline environment. It also provides sufficient silicate and aluminate components to promote efficient geopolymerization, contributing to the formation of a stable three-dimensional aluminosilicate gel network, such as NASH gel. This is fundamental to the high strength of geopolymer gel materials. The appropriate molar ratio of Na₂O, Al₂O₃, SiO₂, and H₂O helps reduce porosity in the slurry, thereby improving the density and compressive strength of the prepared geopolymer. All the following examples follow this ratio.

[0040] The technical solution of the present invention will be further described below through specific embodiments.

[0041] In the following embodiments, unless otherwise specified, the methods described are conventional methods; and unless otherwise specified, the reagents and materials described are commercially available.

[0042] In the following embodiments, the modulus of the alkaline activation solution is the molar ratio of silicon dioxide to sodium oxide in the alkaline activation solution. The specific calculation formula is: Modulus = Molar amount of SiO2 / Molar amount of Na2O.

[0043] The normal temperature condition is 25℃±5℃.

[0044] The main component of dolomite is CaMg(CO3)2. The following examples use 200-350 mesh dolomite produced by Shijiazhuang Mineral Products Factory in Hebei Province. The chemical composition of dolomite is shown in Table 1.

[0045] The metakaolin used in the following examples is 4000 mesh metakaolin produced by Inner Mongolia Chaopai New Materials. The chemical composition of the metakaolin is shown in Table 2.

[0046] Table 1 Chemical composition of dolomite Note: LOI represents the percentage of mass loss of the sample after ignition. Table 2 Chemical composition of metakaolin Example 1 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: Step 1: Preparation of modified alkaline activation solution: 62g of solid sodium hydroxide was mixed thoroughly with 151.28g of water to obtain a sodium hydroxide solution. 86.41g of silicon dioxide was added to 213.28g of the sodium hydroxide solution, and the mixture was stirred for 24 hours to obtain a sodium silicate solution. The modulus of the sodium silicate solution was 1.89, and the mass percentage of sodium silicate in the alkaline-activated solution was 49.49%.

[0047] Sodium silicate solution was used as the alkaline activation solution. The mass ratio of alkaline activation solution to dolomite was 33.1:1. 9.06 g of dolomite was added to 299.69 g of sodium silicate solution, and the mixture was stirred at room temperature for 24 h. The stirring speed during this process was 400 rpm to ensure sufficient reaction between the alkaline activation solution and the dolomite. After the reaction, a sodium silicate-dolomite suspension was obtained, which was used as the modified alkaline activation solution. In the sodium silicate-dolomite suspension, SiO2 and Ca... 2+ With Mg 2+ The molar ratio was 1.89:0.115:0.115; the pH value was 13.46.

[0048] Step 2: Preparation of geopolymer cementitious materials: Using metakaolin as a geopolymer precursor, 308.75g of sodium silicate-dolomite suspension and 181.25g of metakaolin were mixed and stirred at room temperature for 4 minutes to ensure complete and uniform mixing. The mass percentage of dolomite in the geopolymer precursor was controlled to be 5%. The resulting geopolymer cementitious material was denoted as 5DM(SS).

[0049] Example 2 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: Step 1: Preparation of modified alkaline activation solution: 62g of solid sodium hydroxide was mixed thoroughly with 151.28g of water to obtain a sodium hydroxide solution. 86.41g of silicon dioxide was added to 213.28g of the sodium hydroxide solution to obtain a sodium silicate solution. The modulus of the sodium silicate solution was 1.89, and the mass percentage of sodium silicate in the alkaline-activated solution was 49.49%.

[0050] Using sodium silicate solution as the alkali activation solution, and with a mass ratio of alkali activation solution to dolomite of 16.55:1, 18.11 g of dolomite was added to 299.69 g of sodium silicate solution, and the mixture was stirred at room temperature for 24 h. The stirring speed during this process was 400 rpm to ensure sufficient reaction between the alkali activation solution and the dolomite. After the reaction, a sodium silicate-dolomite suspension was obtained, which was used as the modified alkali activation solution. In the sodium silicate-dolomite suspension, SiO2 and Ca... 2+ Mg 2+ The molar ratio was 1.89:0.23:0.23; the pH value was 13.41.

[0051] Step 2: Preparation of geopolymer cementitious materials: Using metakaolin as a geopolymer precursor, 317.81g of sodium silicate-dolomite suspension and 181.25g of metakaolin were mixed and stirred at room temperature for 4 minutes to ensure complete and uniform mixing. The mass percentage of dolomite in the geopolymer precursor was controlled to be 10%. The resulting geopolymer cementitious material was denoted as 10DM(SS).

[0052] Example 3 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: 3.1 g of solid sodium hydroxide was mixed with 37.82 g of water to obtain a sodium hydroxide solution. 9.06 g of dolomite was added to 40.92 g of the sodium hydroxide solution and stirred for 24 h to obtain a sodium hydroxide-dolomite mixed solution. 58.9 g of solid sodium hydroxide was mixed with 86.41 g of silicon dioxide and 113.46 g of water and stirred for 24 h to obtain a sodium silicate solution.

[0053] Add 49.98g of sodium hydroxide-dolomite mixed solution to 258.77g of sodium silicate solution, stir evenly, then add 181.25g of metakaolin, mix and stir for 4 minutes to make it completely uniform, wherein the mass percentage of dolomite as geopolymer precursor is controlled to be 5%; the geopolymer cementitious material is obtained, denoted as 5DM(SH).

[0054] Example 4 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: 3.1 g of solid sodium hydroxide was mixed with 37.82 g of water to obtain a sodium hydroxide solution. 18.12 g of dolomite was added to 40.92 g of the sodium hydroxide solution and stirred for 24 h to obtain a sodium hydroxide-dolomite mixed solution. 58.9 g of solid sodium hydroxide was mixed with 86.41 g of silicon dioxide and 113.46 g of water and stirred for 24 h to obtain a sodium silicate solution.

[0055] Add 49.98g of sodium hydroxide-dolomite mixed solution to 258.77g of sodium silicate solution, stir evenly, then add 181.25g of metakaolin, mix and stir for 4 minutes to make it completely uniform, wherein the mass percentage of dolomite as geopolymer precursor is controlled to be 10%; the geopolymer cementitious material is obtained, denoted as 10DM(SH).

[0056] Example 5 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite differs from Example 3 in that the mass percentage of dolomite in the geopolymer precursor is controlled to 0%, resulting in geopolymer cementitious materials, denoted as ODM(SH).

[0057] Table 3. Raw material ratios for Examples 1 to 4 Note: The amount of dolomite used indicates the percentage of the polymer precursor by mass of dolomite.

[0058] SiO2 and Ca 2+ Mg 2+ The molar ratio indicates the ratio of SiO2 to Ca in the modified alkaline-activated solution. 2+ Mg 2+ The molar ratio.

[0059] Comparative Example 1 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: 62g of solid sodium hydroxide was mixed thoroughly with 151.28g of water to obtain a sodium hydroxide solution. 86.41g of silicon dioxide was added to 213.28g of the sodium hydroxide solution and stirred for 24 hours to obtain a sodium silicate solution. 181.25g of metakaolin and 9.06g of dolomite were thoroughly mixed to obtain a metakaolin-dolomite mixture.

[0060] Using metakaolin as a geopolymer precursor, 190.31g of a metakaolin-dolomite mixture was added to 299.69g of sodium silicate solution and stirred for 4 minutes to ensure complete and uniform mixing. The dolomite constituted 5% of the mass percentage of the geopolymer precursor, resulting in a geopolymer cementitious material, denoted as 5DM.

[0061] Comparative Example 2 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: 62g of solid sodium hydroxide was mixed with 151.28g of water to obtain a sodium hydroxide solution. 86.41g of silicon dioxide was added to 213.28g of the sodium hydroxide solution and stirred for 24 hours to obtain a sodium silicate solution. 181.25g of metakaolin and 18.12g of dolomite were thoroughly mixed to obtain a metakaolin-dolomite mixture.

[0062] Using metakaolin as a geopolymer precursor, 199.37g of a metakaolin-dolomite mixture was added to 299.69g of sodium silicate solution and stirred for 4 minutes to ensure complete and uniform mixing. The dolomite constituted 10% of the mass percentage of the geopolymer precursor, resulting in a geopolymer cementitious material, denoted as 10DM.

[0063] Comparative Example 3 A method for preparing geopolymer cementitious materials based on alkaline solution-modified dolomite includes the following steps: 62g of sodium hydroxide solid was mixed with 151.28g of water to obtain a sodium hydroxide solution; 86.41g of silicon dioxide was added to 213.28g of sodium hydroxide solution and stirred for 24h to obtain a sodium silicate solution.

[0064] Using metakaolin as a geopolymer precursor, 181.25g of metakaolin was added to 299.69g of sodium silicate solution and mixed for 4 minutes to ensure complete and uniform mixing, thus obtaining a geopolymer cementitious material, denoted as MK.

[0065] Table 4. Raw material ratios for Comparative Examples 1 and 2 Note: The amount of dolomite used indicates the percentage of the polymer precursor by mass of dolomite. MK represents the blank control.

[0066] Test 1: The heat of reaction and setting time of the polymer cementitious material were tested.

[0067] Grouping: The geopolymer cementitious material obtained by the method of Example 1 is designated as 5DM(SS); the geopolymer cementitious material obtained by the method of Example 2 is designated as 10DM(SS); the geopolymer cementitious material obtained by the method of Example 3 is designated as 5DM(SH); the geopolymer cementitious material obtained by the method of Example 4 is designated as 10DM(SH); the geopolymer cementitious material obtained by the method of Example 5 is designated as 0DM(SH); the polymer cementitious material obtained by the method of Comparative Example 1 is designated as 5DM; the polymer cementitious material obtained by the method of Comparative Example 2 is designated as 10DM; and the polymer cementitious material obtained by the method of Comparative Example 3 is designated as MK.

[0068] The geopolymer cementitious materials prepared in Examples 1-5 and Comparative Examples 1-3 were transferred into molds, compacted by vibration, and placed in a curing chamber. The heat of reaction and setting time of the geopolymer cementitious materials were tested. The results are as follows: Figures 1-2 As shown in Table 5.

[0069] Table 5. Setting time of geopolymer gel materials Note: Sample number indicates the group of the geopolymer gel material. Setting time is the setting time at a depth of 25 mm. "-" indicates not tested.

[0070] Figure 1 These are the penetration curves of the polymer cementitious materials of Examples 3 to 4 and Comparative Examples 1 to 3 over time. Figure 2 These are the sinking depth curves of the polymer cementitious materials in Examples 1-2 and Comparative Examples 1-3 as a function of time.

[0071] Penetration depth is an indicator of the hardness or softness of a material. For geopolymer materials, penetration depth reflects their degree of curing and hardness. Generally, the smaller the penetration depth, the harder the geopolymer material and the higher its degree of curing. Curing time is a crucial factor affecting the penetration depth of geopolymer materials. As curing time increases, the geopolymer material gradually hardens, its hardness increases, and its penetration depth gradually decreases. This is because during the curing process, internal chemical reactions gradually occur within the geopolymer material, increasing its hardness and strength.

[0072] Figure 1 This study demonstrates the variation in setting time of modified geopolymer slurries under different dolomite addition amounts and with or without sodium hydroxide solution treatment. The results show that compared to the control group (MK group), the setting times of the 5DM and 10DM groups with added unmodified dolomite were prolonged, and the setting time was further delayed with increasing dolomite addition. The initial setting times of the 5DM and 10DM groups were 38 hours and 40.5 hours, respectively, representing delays of 17% and 25% compared to the 32.5 hours of the MK group. The 5DM(SH) and 10DM(SH) groups treated with sodium hydroxide solution exhibited a shortening effect on setting time. Compared with the untreated 5DM and 10DM groups, the setting time of the 5DM(SH) group was 35 hours, and the time shortened by modification accounted for 54.5% of the total retarding time caused by the direct addition of unmodified dolomite; the setting time of the 10DM(SH) group was also 35 hours, and the time shortened by modification accounted for 68.8% of the total retarding time caused by the direct addition of unmodified dolomite.

[0073] Figure 2This study demonstrates the effects of sodium silicate solution treatment and different dolomite addition amounts on the setting time of modified geopolymer slurries. Experimental results show that the setting times of the 5DM(SS) and 10DM(SS) groups treated with sodium silicate solution were shorter than those of the untreated 5DM and 10DM groups. The setting time of the 5DM(SS) group was 34 hours, compared to 38 hours for 5DM. The time reduction due to modification accounted for 72.7% of the total retarding time caused by the direct addition of unmodified dolomite, and its setting curve was highly consistent with that of the MK group. The setting time of the 10DM(SS) group was 35.5 hours, compared to 40.5 hours for 10DM. The time reduction due to modification accounted for 62.5% of the total retarding time caused by the direct addition of unmodified dolomite. This phenomenon indicates that sodium silicate solution treatment effectively shortens the setting time of geopolymers. The reason may be that the sodium silicate solution modification treatment destroys the crystal structure of dolomite, promotes the release of calcium ions, enhances the reactivity of dolomite, and accelerates the reaction process of geopolymers.

[0074] The above analysis shows that when the mass percentage of dolomite in the geopolymer precursor is denoted as k%, and 5 ≤ k < 10, the process of treating dolomite with sodium silicate solution can effectively accelerate the internal chemical reaction rate of the geopolymer material, allowing it to reach the initial setting state in a shorter time. The shortened initial setting time means that the geopolymer material can form a stable structure more quickly, thereby improving construction efficiency.

[0075] The overall penetration depth curve of Example 1 shifted significantly to the left, indicating that under the same curing time, the improved geopolymer material had a smaller penetration depth, i.e., higher hardness. This is because the improvement in the method of Example 1 increased the curing rate and degree of curing of the geopolymer material, enabling it to achieve higher hardness in a shorter time.

[0076] Test 2: Test the mechanical properties of the obtained geopolymer samples.

[0077] The geopolymer cementitious materials prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were transferred into molds, compacted by vibration, placed in a curing chamber, and cured at 20°C for 3 days. After demolding, the samples were cured for 3 days, 7 days, and 28 days, and the mechanical properties of the resulting geopolymer samples were tested.

[0078] Figure 3 This is a comparison chart of the compressive strength of geopolymer samples from Examples 3 to 4 and Comparative Examples 1 to 3 under different curing times.

[0079] Figure 4 This is a comparison chart of the compressive strength of geopolymer samples from Examples 1 to 2 and Comparative Examples 1 to 3 under different curing times.

[0080] Figure 3 The results showed that the compressive strength of the 5DM and 10DM samples was significantly lower than that of the MK samples. This indicates that adding dolomite directly to the geopolymer results in increased setting time, slow strength growth, and decreased strength in the later stages of the polymer sample preparation.

[0081] like Figure 3 Compared with the 5DM and 10DM samples, the dolomite treated with sodium hydroxide solution in the 5DM(SH) and 10DM(SH) samples showed a significant improvement in compressive strength.

[0082] like Figure 4 Compared with the 5DM and 10DM samples, the dolomite treated with sodium silicate solution in the 5DM(SS) and 10DM(SS) samples showed a significant improvement in compressive strength.

[0083] Compared to the 5DM(SH) and 10DM(SH) samples, the 5DM(SS) sample exhibited significantly higher compressive strength. This indicates that the method in Example 1 can significantly improve the later-stage compressive strength. However, with the increase of dolomite content, the compressive strength of the material decreased. Therefore, the method of this embodiment, by treating dolomite with sodium silicate solution and controlling the mass percentage of dolomite in the polymer precursor to 5 wt%, can significantly improve the compressive strength of the material.

[0084] Test 3: Effect of alkaline activation solution on the concentration of dissolved ions in dolomite.

[0085] The ion concentration of the sodium silicate solution was determined, and the results are as follows: Figure 5 As shown. The ion concentration of the sodium hydroxide solution-modified solution was determined, and the results are as follows. Figure 6 As shown.

[0086] Figure 5 The results show the concentration of dissolved ions in the polymer gelling materials of Examples 1, 2, and Comparative Example 3.

[0087] Figure 6 The results are for the determination of leached ion concentrations of the polymer gelling materials in Examples 3 and 4 and Comparative Example 3.

[0088] from Figure 5 It can be clearly seen that a certain amount of calcium and magnesium ions are indeed present in the solution. With the gradual increase of dolomite addition, the concentrations of these two ions show a linear increasing trend. Specifically, when the amount of dolomite added doubles, the concentrations of calcium and magnesium ions increase by 65.8% and 66.3%, respectively. The high similarity between these two growth rates further confirms that the calcium and magnesium ions do indeed originate from the reaction between dolomite and hydroxide ions, and that their release process is stable and predictable.

[0089] Investigating the effects of these ions on the coagulation process of metakaolin polymers reveals that calcium ions significantly accelerate the coagulation process of metakaolin polymers, neglecting pH changes. Free calcium ions in solution facilitate the early formation of calcium aluminum silicate hydrate (CASH), thereby accelerating the reaction process, while magnesium ions shorten the coagulation time through multiphase nucleation by providing nucleation sites in the initial slurry solution.

[0090] It is hypothesized that the reaction between dolomite and hydroxide ions involves two potential pathways, the first of which involves the formation of calcium and magnesium ions in solution. To verify this hypothesis, inductively coupled plasma (ICP-C) testing technology was used in this embodiment of the invention to accurately measure the concentrations of calcium and magnesium ions in each group of solutions. The results are as follows: Figure 6 As shown.

[0091] like Figure 6 Since the compositions of the MK, 5DM, and 10DM solutions were identical, DM was used to represent this group of solutions in subsequent analyses for ease of comparison and discussion. ICP testing revealed that although the concentrations of calcium and magnesium ions in the solutions were low, they were indeed present, and their concentrations increased with increasing dolomite content. This finding directly proves that a reaction did occur between dolomite and hydroxide ions, generating calcium and magnesium ions. When the dolomite content increased from 5 wt% to 10 wt%, the concentrations of calcium and magnesium ions increased by 18.4% and 238.5%, respectively.

[0092] In summary, the present invention, through treating dolomite with sodium silicate solution and controlling the mass percentage of dolomite in the geopolymer precursor to 5 wt%, can improve the reactivity of dolomite, shorten the solidification time of the geopolymer material, increase the sinking depth and compressive strength of the geopolymer material, and realize the high-value utilization of low-value dolomite materials.

[0093] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a geopolymer cementitious material based on dolomite modified by an alkaline solution, characterized in that, The method comprises the following steps: The alkali-activated solution is mixed with dolomite to obtain a modified alkali-activated solution; in the modified alkali-activated solution, the molar ratio of SiO2, Ca 2+ , and Mg 2+ is 1.9:0.1-0.3:0.1-0.

3. Mixing and stirring the modified alkali-activated solution with the geopolymer precursor to obtain a geopolymer cementing material; the mass percentage of dolomite in the geopolymer precursor is 5-10%.

2. The method for producing geopolymer cementitious material based on alkaline solution modified dolomite according to claim 1, characterized in that, The alkali-activated solution is a silicate solution, and the modulus of the silicate solution is 1.5-2.

3. The method for producing geopolymer cementitious material based on alkaline solution modified dolomite according to claim 1, characterized in that, The modulus of the silicate solution is 1.8-1.

9.

4. The method for producing geopolymer cementitious material based on modified dolomite with alkaline solution according to claim 2, characterized in that, The alkali-activated solution is a sodium silicate solution or a potassium silicate solution.

5. The method for producing geopolymer cementitious material based on alkaline solution modified dolomite according to claim 1, characterized in that, The mixing time of the alkali-activated solution and the dolomite is 24 h.

6. The method for producing geopolymer cementitious material based on alkaline solution modified dolomite according to claim 1, characterized in that, The pH of the modified alkali-activated solution is 13-14.

7. The method for producing geopolymer cementitious material based on alkaline solution modified dolomite according to claim 1, characterized in that, The geopolymer precursor is metakaolin or fly ash.

Citation Information

Cited By

  • Dolomite-based carbonizable cementing material as well as preparation method and application thereof

    CN122254785A