Silicon carbide powder preparation device

By using denitrified metal powder in a denitrification container for heating and adsorption in a silicon carbide powder preparation device, the problems of thermal corrosion and impurity introduction caused by hydrogen gas were solved, achieving the preparation of high-purity silicon carbide powder, reducing power load and improving particle size control.

CN121060397APending Publication Date: 2025-12-05JIANG SU JI XIN XIAN JIN CAI LIAO YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511160093.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-19
Publication Date
2025-12-05

AI Technical Summary

Technical Problem

In the existing technology for synthesizing high-purity silicon carbide powder, the increase in hydrogen gas leads to intensified thermal corrosion, increased power load, unsatisfactory denitrification and particle size control, and the introduction of metallic powder impurities, which affects the purity of silicon carbide powder.

Method used

The process involves filling a denitrification container with denitrification metal powder, heating the powder to perform physical and chemical adsorption, removing nitrogen from the gas phase components, reducing hydrogen usage, avoiding thermal corrosion and impurity introduction, and controlling the synthesis process using inert gas and heating devices.

Benefits of technology

It improves the purity of silicon carbide powder, reduces power load, avoids thermal corrosion, and achieves better particle size control and manageability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121060397A_ABST
    Figure CN121060397A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon carbide powder preparation device, which comprises: a reaction container, which is provided with an inert gas inlet and an extraction opening; the interior of the synthesis container is suitable for synthesizing silicon carbide powder from carbon powder and silicon powder, and the synthesis container is arranged in the reaction container; nitrogen removal metal powder is contained in the nitrogen removal container, the nitrogen removal container is arranged in the reaction container, and the nitrogen removal container and the synthesis container are arranged in a spaced mode; and the heating device is suitable for heating the reaction container. The silicon carbide powder preparation device has the advantages of being high in preparation purity, small in power load, not prone to corrosion, good in controllability and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicon carbide preparation technology, and more specifically, to a silicon carbide powder preparation apparatus. Background Technology

[0002] In the process of growing silicon carbide crystals by physical vapor transport (PVT), the purity requirements of silicon carbide powder are particularly important for the growth of high-purity silicon carbide crystals. The impurity concentration of silicon carbide powder, such as nitrogen content, directly affects the resistivity of high-purity crystals.

[0003] In the synthesis of high-purity silicon carbide powder in related technologies, a relatively high synthesis temperature is used, and argon and hydrogen are introduced during the synthesis process to reduce the nitrogen content in the reaction. However, during the gas introduction process, as the proportion of hydrogen in the mixed gas increases, hydrogen has a significant impact on the thermal insulation performance. At high temperatures, this leads to accelerated thermal corrosion, increased power load during synthesis, and decreased temperature, resulting in unsatisfactory denitrification and particle size control. Summary of the Invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a silicon carbide powder preparation device, which has the advantages of high purity, low power load, resistance to corrosion, and good controllability.

[0005] To achieve the above objectives, an apparatus for preparing silicon carbide powder is provided according to an embodiment of the present invention. The apparatus includes: a reaction vessel having an inert gas inlet and an exhaust port; a synthesis vessel suitable for synthesizing silicon carbide powder from carbon powder and silicon powder, the synthesis vessel being disposed within the reaction vessel; a denitrification vessel containing denitrified metal powder, the denitrification vessel being disposed within the reaction vessel, the denitrification vessel being spaced apart from the synthesis vessel; and a heating device adapted to heat the reaction vessel.

[0006] The silicon carbide powder preparation apparatus according to embodiments of the present invention has advantages such as high purity, low power load, resistance to corrosion, and good controllability.

[0007] In addition, the silicon carbide powder preparation apparatus according to the above embodiments of the present invention may also have the following additional technical features:

[0008] According to one embodiment of the present invention, the denitrification container is disposed above the synthesis container, the extraction port is located at the upper part of the reaction container and the inert gas inlet is disposed at the lower part of the reaction container.

[0009] According to one embodiment of the present application, the reaction container is provided with a carrier plate, which separates the reaction container into an upper chamber and a lower chamber, and a gas outlet is provided on the carrier plate, the nitrogen removal container is arranged in the upper chamber and the synthesis container is arranged in the lower chamber, the gas outlet is communicated with the upper chamber and the inert gas inlet is communicated with the lower chamber.

[0010] According to one embodiment of the present application, the heating device comprises a side heating device arranged outside the circumferential wall of the lower chamber and a bottom heating device arranged below the bottom wall of the reaction container.

[0011] According to one embodiment of the present application, the silicon carbide powder preparation device further comprises an outer container arranged outside the reaction container, a heat preservation layer arranged between the outer container and the reaction container, and the heating device is arranged between the heat preservation layer and the reaction container, and an outer gas outlet is arranged on the outer container.

[0012] According to one embodiment of the present application, an annular support block is arranged on the inner bottom surface of the reaction container, the synthesis container is arranged on the annular support block, the inert gas inlet is arranged on the bottom wall of the reaction container and located radially inside the annular support block, and a temperature measuring port is further arranged on the bottom wall of the reaction container and located radially inside the annular support block.

[0013] According to one embodiment of the present application, the nitrogen removal metal powder is titanium powder.

[0014] According to one embodiment of the present application, the nitrogen removal container is made of graphite material.

[0015] According to one embodiment of the present application, the heating device comprises a nitrogen removal powder heating device, which extends into the nitrogen removal container, the nitrogen removal container is made of copper material, a cooling pipeline is wound outside the nitrogen removal container, and the cooling pipeline is communicated with a cooling liquid source.

[0016] According to one embodiment of the present application, the heating device is adapted to heat the nitrogen removal metal powder to a molten state.

[0017] Additional aspects and advantages of the present application will be in part apparent and in part pointed out hereinafter. BRIEF DESCRIPTION OF DRAWINGS

[0018] The above and / or additional aspects and advantages of the present application will become apparent and be readily understood from the following description, taken in conjunction with the accompanying drawings, in which:

[0019] Figure 1is a sectional view of a silicon carbide powder preparation device according to one embodiment of the present application.

[0020] Figure 2 is a sectional view of a silicon carbide powder preparation device according to another embodiment of the present application.

[0021] Fig. 1 is a sectional view of a silicon carbide powder preparation device according to one embodiment of the present application. DETAILED DESCRIPTION

[0022] The present application is based on the discovery and realization of the following facts and problems:

[0023] In the synthesis process of high-purity silicon carbide powder in the related art, a higher synthesis temperature is adopted and argon and hydrogen are introduced during the synthesis process, and the content of nitrogen element in the reaction process is reduced by using hydrogen. However, during the gas introduction process, with the increase of the proportion of hydrogen in the mixed gas, hydrogen has a great influence on the heat field insulation performance, and at high temperature, it can cause the corrosion of the heat field to be intensified, the power load in the synthesis process to be increased, and the temperature to be reduced, resulting in that the denitrogenation effect and the particle size control are not ideal.

[0024] Specifically, in the synthesis method of high-purity silicon carbide powder in the related art, by adding denitrogenation metal powder to carbon powder and silicon powder raw materials, physical and chemical adsorption of nitrogen element is carried out to reduce the content of nitrogen, but metal powder impurities are inevitably introduced into silicon carbide, which also causes the purity of the synthesized silicon carbide powder to be reduced.

[0025] Embodiments of the present application are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements having the same or similar functions throughout. The embodiments described below by referring to the drawings are exemplary and are only used to explain the present application, and cannot be understood as a limitation of the present application.

[0026] In the description of the present application, it is to be understood by the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, which are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a particular orientation, be constructed and operated in a particular orientation, and therefore cannot be understood as limiting the present application. In addition, the features defined as "first", "second" can be explicitly or implicitly include one or more of the features. In the description of the present application, unless otherwise specified, the meaning of "a plurality of" is two or more.

[0027] In the description of the present application, it should be noted that unless otherwise specified and limited, the terms "mounting", "connecting", "connecting" should be understood broadly, for example, it can be fixedly connected, or it can be detachably connected, or integrally connected; it can be mechanically connected, or it can be electrically connected; it can be directly connected, or it can be indirectly connected through an intermediate medium, and it can be the communication between the two elements inside. For those skilled in the art, the specific meaning of the above terms in the present application can be understood according to the specific circumstances.

[0028] The silicon carbide powder preparation device 1 according to the embodiment of the present application is described below with reference to the drawings.

[0029] As shown in Figure 1 and Figure 2 The silicon carbide powder preparation device 1 according to the embodiment of the present application includes a reaction vessel 10, a synthesis vessel 20, a nitrogen removal vessel 30 and a heating device.

[0030] The reaction vessel 10 is provided with an inert gas inlet 11 and an exhaust port 12. The synthesis vessel 20 is suitable for synthesizing silicon carbide powder from carbon powder and silicon powder, and is arranged in the reaction vessel 10. The nitrogen removal vessel 30 contains nitrogen removal metal powder 31, and is arranged in the reaction vessel 10, with the nitrogen removal vessel 30 being spaced apart from the synthesis vessel 20. The heating device is suitable for heating the reaction vessel 10.

[0031] Specifically, the reaction container 10 can be a graphite reaction kettle. The synthesis container 20 can be a crucible, and the synthesis container 20 is filled with the powder 2, and the silicon powder and the carbon powder are mixed and synthesized into the silicon carbide powder in the synthesis container 20. The gas outlet 12 is suitable for extracting the gas in the reaction container 10 to achieve a high vacuum environment and to achieve pressure control in the reaction container 10. The nitrogen removal container 30 is in gas communication with the reaction container 10, for example, the upper surface of the nitrogen removal container 30 can be open. The inert gas inlet 11 can be connected to inert gas and hydrogen.

[0032] First, the mixed powder 2 of the carbon powder and the silicon powder is loaded into the synthesis container 20, and the nitrogen removal metal powder 31 is loaded into the nitrogen removal container 30. Then, the gas outlet 12 extracts the gas to form a high vacuum environment in the reaction container 10. The inert gas is introduced through the inert gas inlet 11. Then the heating device is used to heat the nitrogen removal metal powder 31, and the nitrogen element in the reaction container 10 is fully consumed by controlling the temperature rise and temperature maintenance during the process. Finally, the synthesis container 20 is heated to the synthesis temperature for synthesis.

[0033] According to the silicon carbide powder preparation device 1 of the embodiment of the present application, by arranging the nitrogen removal container 30 and loading the nitrogen removal metal powder 31 in the nitrogen removal container 30, the nitrogen element can be physically and chemically adsorbed by the nitrogen removal metal powder 31 during the heating process before the synthesis reaction starts, and the nitrogen element in the gas phase component is removed, thereby reducing the content of nitrogen impurities in the synthesis process and improving the purity of the synthesized silicon carbide powder.

[0034] Furthermore, by arranging the nitrogen removal container 30 and loading the nitrogen removal metal powder 31 in the nitrogen removal container 30, compared with the technical solution of completely using hydrogen to reduce the content of nitrogen element in the related art, the need for hydrogen can be reduced, the influence of hydrogen on the heat field insulation performance can be avoided, the corrosion of hydrogen can be avoided, the power load of the heating device in the synthesis process can be reduced, and the particle size of the synthesized silicon carbide can be controlled.

[0035] In addition, by arranging the nitrogen removal container 30 to be spaced from the synthesis container 20 in the reaction container 10, not only the nitrogen element in the gas phase component of the reaction container 10 can be removed by the nitrogen removal metal powder 31 in the nitrogen removal container 30, but also the nitrogen removal metal powder 31 can be prevented from mixing into the powder 2 in the synthesis container 20, compared with the technical solution of directly adding the nitrogen removal powder to the raw material powder in the related art, other impurities can be prevented from mixing into the silicon carbide, and the purity of the silicon carbide powder can be further improved.

[0036] Therefore, the silicon carbide powder preparation device 1 according to the embodiment of the present application has the advantages of high purity, small power load, not easy to corrode, good controllability, etc.

[0037] The silicon carbide powder preparation device 1 according to the embodiment of the present application will be described below with reference to the accompanying drawings.

[0038] In some embodiments of the present application, as shown in Figure 1 and Figure 2 , the silicon carbide powder preparation device 1 according to the embodiments of the present application comprises a reaction container 10, a synthesis container 20, a denitrogenation container 30 and a heating device.

[0039] Advantageously, as shown in Figure 1 and Figure 2 , the denitrogenation container 30 is arranged above the synthesis container 20 (the up-down direction is shown by the arrow in the figure), the air outlet 12 is arranged at the upper part of the reaction container 10 and the inert gas inlet 11 is arranged at the lower part of the reaction container 10. In this way, the gas flow can flow from bottom to top, and the gas flow first passes through the synthesis container 20 and then passes through the denitrogenation container 30, so as to avoid the gas flow carrying the denitrogenation metal powder 31 in the denitrogenation container 30 into the powder 2 in the synthesis container 20, thereby further facilitating the improvement of the purity of the silicon carbide.

[0040] More advantageously, as shown in Figure 1 and Figure 2 , the reaction container 10 is provided with a carrier disc 50, the carrier disc 50 separates the reaction container 10 into an upper chamber 13 and a lower chamber 14, the carrier disc 50 is provided with a gas passage 51, the denitrogenation container 30 is arranged in the upper chamber 13 and the synthesis container 20 is arranged in the lower chamber 14, the air outlet 12 is in communication with the upper chamber 13, and the inert gas inlet 11 is in communication with the lower chamber 14. Specifically, the carrier disc 50 can be a graphite piece to improve the heat resistance. In this way, not only can the gas flow flow in the direction from the lower chamber 14 to the upper chamber 13, so that the gas flow first passes through the synthesis container 20 and then passes through the denitrogenation container 30, but also the separation of the denitrogenation container 30 and the synthesis container 20 can be further facilitated, and the mixing of the denitrogenation metal powder 31 impurities into the silicon carbide powder can be further avoided.

[0041] Specifically, as shown in Figure 1 and Figure 2 , the heating device comprises a side heating device 41 and a bottom heating device 42. The side heating device 41 is arranged outside the peripheral wall of the lower chamber 14. The bottom heating device 42 is arranged below the bottom wall of the reaction container 10. In this way, the reaction container 10 can be heated, the synthesis temperature can be controlled, the temperature gradient in the up-down direction of the reaction container 10 can be controlled, and the temperature of the denitrogenation container 30 can be lower than that of the synthesis container 20 during the heating process.

[0042] More specifically, as shown in Figure 1 and Figure 2 , the side heating device 41 comprises a plurality of side heating elements 41 arranged in the circumferential direction of the lower chamber 14.As shown, the silicon carbide powder preparation device 1 further comprises an outer container 60, which is arranged outside the reaction container 10, and a heat insulation layer 61 is arranged between the outer container 60 and the reaction container 10. The heating device is arranged between the heat insulation layer 61 and the reaction container 10, and an outer exhaust port 62 is arranged on the outer container 60. Specifically, the outer container 60 can be a furnace body, and the outer container 60 can have a cooling water interlayer in the wall to improve the heat resistance of the outer container 60. The heat insulation layer 61 can be a graphite heat insulation felt to improve the heat resistance. In this way, the heat loss of the heating device to the outside can be reduced, the energy consumption of the heating device can be saved, the heating efficiency can be improved, the temperature of the reaction container 10 can be controlled, the outer exhaust port 62 can facilitate the formation of a high-vacuum environment in the outer container 60, the influence of the nitrogen element in the gas phase component on the synthesis process can be reduced, and the pressure control can be facilitated.

[0043] Further, as shown in Figure 1 and Figure 2 , an annular support block 70 is arranged on the inner bottom surface of the reaction container 10, and the synthesis container 20 is arranged on the annular support block 70. The inert gas inlet 11 is arranged on the bottom wall of the reaction container 10 and located radially inside the annular support block 70. A temperature measuring port 15 is also arranged on the bottom wall of the reaction container 10 and located radially inside the annular support block 70. In this way, the gas can enter the reaction container 10 more easily, and the temperature measuring device can more easily access the synthesis container 20, facilitating temperature measurement of the synthesis container 20.

[0044] Specifically, as shown in Figure 1 and Figure 2 , the inert gas inlet 11, the exhaust port 12, and the temperature measuring port 15 are formed on an inert gas pipe, an exhaust pipe, and a temperature measuring pipe, respectively. The inert gas pipe, the exhaust pipe, and the temperature measuring pipe are connected to the reaction container 10. The heating device is connected to an electrode, and the outer container 60 is provided with an opening for avoiding the inert gas pipe, the exhaust pipe, the temperature measuring pipe, and the electrode. A sealing element is arranged in the opening to improve the sealing performance of the outer container 60.

[0045] Optionally, the nitrogen-removing metal powder 31 is titanium powder. Since titanium has a high melting point and a high saturated vapor pressure, titanium powder can be further avoided from being mixed into the silicon carbide synthesis process, which further facilitates the reduction of the impurity content of the silicon carbide powder and the improvement of the purity of the silicon carbide powder.

[0046] Further, the heating device is adapted to heat the nitrogen-removing metal powder 31 to a molten state. In this way, the nitrogen-removing metal powder 31 can react violently with the nitrogen element, improving the removal effect of the nitrogen element impurity content in the gas phase component.

[0047] In some embodiments, as shown in Figure 1 , the nitrogen-removing container 30 is made of graphite material. In this way, the nitrogen-removing container 30 can have good heat resistance.

[0048] Specifically, the powder 2 obtained by mixing 24 kg of high-purity carbon powder and 56 kg of high-purity silicon powder is loaded into the synthesis container 20 at a distance of 100 mm from the upper edge of the synthesis container 20, the synthesis temperature is 2150-2250 °C, the synthesis time at the above-mentioned synthesis temperature range is 50 h, and the synthesis pressure is 80 mbar.

[0049] Reference will now be made to the drawings Figure 1 The synthesis process according to some embodiments of the present application is described as follows:

[0050] Synthesis of hot field and cavity pretreatment: The titanium metal powder with a purity of 99.995% is loaded into the nitrogen removal container 30. The particle size of the titanium metal powder is 2 mm x 2 mm. The nitrogen removal container 30 loaded with the titanium metal powder is placed at the center position of the carrier disc 50. The assembled outer container 60 is sealed.

[0051] At the same time, the two-way vacuum system of the gas extraction port 12 and the outer gas extraction port 62 is started to obtain high vacuum. The process time is 2 h 30 min. After vacuum is obtained, the process is started. After leak detection, argon is introduced through the inert gas inlet 11 after the leak detection is passed, the backfill pressure is 500-800 mbar, and the temperature rising process is started.

[0052] In the first stage, the temperature is raised to 800 °C at a rate of about 200 °C / h. During the temperature rising stage, the argon flow is continuously at a high flow rate of 5000 seem. The pressure of the outer container 60 is maintained at 500 mbar. The two-way vacuum system is continuously operated. It takes about 4 h to raise the temperature to 800 °C in this stage.

[0053] In the second stage, the temperature is controlled at 800 °C for 1 h 30 min. In the first 30 min, the flow rate is reduced to 500 seem. The two-way vacuum system is continuously operated. No pressure control is provided. High vacuum is obtained. Before the end of the first 30 min, the argon flow rate is restored to 5000 seem. The pressure of the outer container 60 is controlled to 500 mbar. This cycle is repeated for 3 times.

[0054] In the third stage, the temperature is raised to 2060-2080 °C (the bottom temperature of the reaction container 10 is monitored through the temperature measuring port 15). The temperature rising rate is 200 °C / h. During the temperature rising stage, the argon flow rate is 1000 seem. Hydrogen is introduced through the inert gas inlet 11. The hydrogen flow rate is 20 seem. The pressure of the outer container 60 is maintained at 500 mbar. The two-way vacuum system is continuously operated. It takes about 6 h to raise the temperature to 2080 °C in this stage.

[0055] In the fourth stage, the temperature is raised to 2150-2250 °C (the bottom temperature of the reaction container 10 is monitored through the temperature measuring port 15). The temperature rising rate is 100 °C / h. During the temperature rising stage, the argon flow rate is 200 seem. The hydrogen flow rate is 10 seem. The pressure of the reaction container 10 is reduced to 80 mbar. The two-way vacuum system is continuously operated. It takes about 1 h to raise the temperature to 2250 °C in this stage.

[0056] The fifth stage is temperature control at 2190-2230 °C (the temperature at the bottom of the reaction container 10 is monitored by the temperature measuring port 15, and the actual temperature in the synthesis container 20 is controlled at 2150 °C). The argon flow is 200 sccm, the hydrogen flow is 10 sccm, the synthesis pressure in the reaction container 10 is 80 mbar, and the two-way vacuum system is continuously operated. This synthesis stage lasts for 50 h.

[0057] The sixth stage is temperature reduction and cooling.

[0058] Specifically, the titanium powder and nitrogen element start to effectively react when the temperature is raised to 800 °C in the first stage. After the end of the second stage, the temperature at the top of the actual reaction container 10 also reaches above 1700 °C during the temperature raising to 2060-2080 °C. In addition to the titanium powder in the nitrogen container 30 starting to be heated, the metal titanium particles gradually melt as the temperature rises after reaching the melting point of about 1700 °C. In the 6 h of the third stage, the heated and even molten metal titanium reacts with nitrogen at high temperature, consumes and absorbs the adsorbed nitrogen in the cavity and heat field. The molten titanium will react violently with the nitrogen element to generate titanium nitride (Ti3N, TiN, etc.) and Ti-N solid solution form, and fully consume the adsorbed nitrogen in the cavity and heat field.

[0059] In other embodiments, as shown in Figure 2 Specifically, the inlet and outlet of the cooling pipeline 80 extend out of the reaction container 10 and the outer container 60 to facilitate connection to the cooling liquid source. In this way, the copper material of the nitrogen removal container 30 can be cooled by the cooling pipeline 80, improving the heat resistance of the nitrogen removal container 30, and the temperature of the nitrogen removal metal powder 31 can be independently controlled, allowing the nitrogen removal process and the synthesis process to be carried out independently, avoiding the mixing of nitrogen removal metal powder 31 impurities in the silicon carbide, and using copper material can effectively improve the sealing performance of the nitrogen removal container 30, further avoiding the leakage of nitrogen removal metal powder 31 into the synthesis container 20, avoiding the mixing of nitrogen removal metal powder 31 impurities in the silicon carbide, and further improving the purity of the silicon carbide powder.

[0060] Specifically, the mixed powder 2 of 56 kg of high-purity silicon powder and 24 kg of high-purity carbon powder is loaded 100 mm away from the upper edge of the synthesis container 20, the synthesis temperature is 2150-2250 °C, the synthesis time at the above synthesis temperature is 50 h, and the synthesis pressure is 80 mbar.

[0061] The synthesis process according to other specific embodiments of the present application is described below with reference to Figure 2

[0062] ​Synthesis of hot field and cavity pretreatment: The purity of 99.995% of the metal titanium powder is loaded into the nitrogen removal container 30 of copper material. The particle size of the metal titanium powder is 2mm x 2mm. The titanium powder loaded nitrogen removal container 30 is placed in the center of the upper chamber 13. The assembled outer container 60 is sealed.

[0063] At the same time, the two-way vacuum system of the exhaust port 12 and the outer exhaust port 62 is started, and high vacuum is obtained. The process time is 2h30min, and after vacuum is obtained, the process leak detection is started, and after the leak detection is passed, argon is introduced, the backfill pressure is 500-800mbar, and the temperature rising process is started.

[0064] The first stage is heated to 800℃ by the side heating device 41 and the bottom heating device 42, and the heating rate is about 200℃ / h. During the heating stage, the argon flow is continuously 5000sccm, the outer container 60 pressure is maintained at 500mbar, and the two-way vacuum system is continuously running. In this stage, the temperature is raised to 800℃ for about 4h. At the same time, the cooling pipeline 80 and the nitrogen removal container 30 with cooling circulating water are always maintained at 24-26℃. The nitrogen removal metal powder 31 in the nitrogen removal container 30 is always in an unheated state.

[0065] The second stage is 800℃ temperature control for 1h30min, and the flow is reduced to 500sccm in the first 30min. The two-way vacuum system is continuously running, and there is no pressure control. High vacuum is obtained, and before the first 30min ends, the argon flow is restored to 5000sccm, and the outer container 60 is controlled to 500mbar. This cycle is repeated 3 times. At the same time, when the temperature control starts, the nitrogen removal powder heating device 43 is started, and the titanium powder in the nitrogen removal container 30 is heated to a molten state. During the 3 times of cycle, the nitrogen removal powder heating device 43 is always started, and the metal titanium powder is always in a "violent combustion" or molten state. In this stage, the reaction principle of the heated "violent combustion" or even molten metal titanium with nitrogen at high temperature is used to consume and absorb the adsorbed nitrogen in the cavity and the hot field. At the same time, the vacuum system of the exhaust port 12 of the reaction container 10 timely removes the reaction gas. After the second stage is about to end, the nitrogen removal powder heating device 43 is stopped, the metal titanium is gradually cooled to 24-26℃ through the cooling pipeline 80, and it is restored to room temperature to achieve a stable state, so as to reduce the introduction of other impurities in the silicon carbide powder synthesis stage. In the subsequent stage, the cooling pipeline 80 always has strong cooling water, and the room temperature stability is maintained.

[0066] The third stage is heated to 2060-2080℃ (the temperature of the bottom of the reaction container 10 is monitored through the temperature measuring port 15), and the heating rate is 200℃ / h. During the heating stage, the argon flow is 1000sccm, and the hydrogen flow is 20sccm. The outer container 60 pressure is maintained at 500mbar, and the two-way vacuum system is continuously running. In this stage, the temperature is raised to 2080℃ for about 6h.

[0067] The fourth stage is to heat to 2150-2250°C (monitoring the temperature of the bottom of the reaction container 10 through the temperature measuring hole 15), the heating rate is 100°C / h, the argon flow rate is 200sccm, the hydrogen flow rate is 10sccm, the pressure of the reaction container 10 is reduced to 80mbar, and the two-way vacuum system is continuously operated. The temperature is heated to 2250°C for about 1h in this stage.

[0068] The fifth stage is to control the temperature at 2190-2230°C (monitoring the temperature of the bottom of the reaction container 10 through the temperature measuring hole 15, and the actual temperature of the synthesis container 20 is controlled at 2150°C), the argon flow rate is 200sccm, the hydrogen flow rate is 10sccm, the synthesis pressure of the reaction container 10 is 80mbar, and the two-way vacuum system is continuously operated. This synthesis stage lasts for 50h.

[0069] The sixth stage is to cool down.

[0070] After the synthesis powder taken out from the furnace in Example 2 is subjected to acid washing, alkali washing, pure water cleaning and drying, the sample is detected for element purity by glow discharge mass spectrometry (GDMS) and secondary ion mass spectrometry (SIMS), as shown in the following table, which completely meets the growth requirements of semi-insulating silicon carbide crystals.

[0071]

[0072]

[0073]

[0074] Other configurations and operations of the silicon carbide powder preparation device 1 according to the embodiments of the present application are known to those skilled in the art, and will not be described in detail here.

[0075] In the description of the present specification, the description of the terms "one embodiment", "some embodiments", "exemplary embodiment", "example", "specific example", or "some examples" and the like means that the specific features, structures, materials or characteristics described in connection with the embodiment or example are included in at least one embodiment or example of the present application. In the present specification, the exemplary description of the above terms does not necessarily mean the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0076] Although the embodiments of the present application have been shown and described, those skilled in the art can understand that various changes, modifications, replacements and variations can be made to the embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the claims and their equivalents.

Claims

1. A silicon carbide powder production apparatus characterized by comprising: The application relates to a reaction container, which comprises: a reaction container provided with an inert gas inlet and an exhaust outlet; a synthesis container, which is adapted to synthesize silicon carbide powder from carbon powder and silicon powder, and is arranged in the reaction container; a nitrogen removal container, which contains nitrogen removal metal powder, is arranged in the reaction container, and is spaced apart from the synthesis container; a heating device, which is adapted to heat the reaction container.

2. The apparatus of claim 1, wherein, The nitrogen removal container is arranged above the synthesis container, the exhaust outlet is arranged at the upper portion of the reaction container, and the inert gas inlet is arranged at the lower portion of the reaction container.

3. The apparatus of claim 1, wherein, The reaction container is provided with a carrier disc, which divides the reaction container into an upper chamber and a lower chamber, and is provided with a gas passage, the nitrogen removal container is arranged in the upper chamber, the synthesis container is arranged in the lower chamber, the exhaust outlet is communicated with the upper chamber, and the inert gas inlet is communicated with the lower chamber.

4. The apparatus of claim 3, wherein the carbonization chamber is a graphite crucible. The heating device comprises: a side heating device, which is arranged outside the peripheral wall of the lower chamber; a bottom heating device, which is arranged below the bottom wall of the reaction container.

5. The apparatus of claim 1, wherein The application further comprises an outer container, which is arranged outside the reaction container, is provided with a heat insulation layer between the reaction container and the outer container, and is provided with an outer exhaust outlet.

6. The apparatus of claim 1, wherein, The reaction container is provided with an annular support block on the inner bottom surface, the synthesis container is arranged on the annular support block, the inert gas inlet is arranged on the bottom wall of the reaction container and is located inside the annular support block in the radial direction, and the bottom wall of the reaction container is further provided with a temperature measuring opening, which is located inside the annular support block in the radial direction.

7. The apparatus of claim 1, wherein, The nitrogen removal metal powder is titanium powder.

8. The apparatus of claim 1, wherein, The nitrogen removal container is made of graphite material.

9. The apparatus of claim 1, wherein, The heating device comprises a nitrogen removal powder heating device, which extends into the nitrogen removal container, the nitrogen removal container is made of copper material, the nitrogen removal container is provided with a cooling pipeline, and the cooling pipeline is communicated with a cooling liquid source.

10. The apparatus of claim 1, wherein, The heating device is adapted to heat the nitrogen removal metal powder to a molten state.