Directional Wetting Gradient Assembled Solar Evaporator, Its Preparation Method and Application

By designing an assembled solar evaporator with a directional wettability gradient, the problem of oil and salt clogging in petrochemical wastewater was solved, achieving efficient separation and dynamic equilibrium evaporation treatment of oil and salt wastewater, improving treatment efficiency and reducing energy consumption.

CN121085356BActive Publication Date: 2026-11-10TIANJIN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511240968.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-09-02
Publication Date
2026-11-10
Estimated Expiration
2045-09-02

AI Technical Summary

Technical Problem

Existing solar-driven interfacial evaporation technology suffers from reduced evaporation efficiency due to oil blockage and salt accumulation when treating petrochemical wastewater. Furthermore, it lacks sufficient resistance to oil and salt, making it difficult to effectively separate complex oil and salt wastewater.

Method used

Design an assembled solar evaporator with a directional wettability gradient, including an oil-blocking layer, a low-wetting water transport layer, and a high-wetting salt-blocking layer. The wettability gradient guides water transport, avoids oil and salt blockage, and achieves oil and salt separation.

Benefits of technology

It achieves efficient graded purification of petrochemical wastewater, separating oil and leaving salt residue. During the evaporation process, a dynamic balance between water transport and evaporation is maintained, improving treatment efficiency and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121085356B_ABST
    Figure CN121085356B_ABST
Patent Text Reader

Abstract

This invention relates to the field of oil-resistant and wastewater treatment technology, specifically to a directional wettability gradient-assembled solar evaporator, its preparation method, and its application. The invention provides a directional wettability gradient-assembled solar evaporator, comprising, from bottom to top, an oil-blocking layer, a low-wetting water-transporting layer, and a high-wetting salt-barrier layer. The wettability relationship between these layers is: the oil-blocking layer is greater than the low-wetting water-transporting layer, and the low-wetting water-transporting layer is less than the high-wetting salt-barrier layer. This invention innovatively proposes the concept of a modular evaporator, characterized by a wettability gradient, which can be used for the staged purification of petrochemical wastewater. It solves the problem of performance degradation of SDIE (Synthetic Evaporator for Petrochemical Wastewater Treatment) due to oil blockage and salt accumulation when treating petrochemical wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of oil-resistant and wastewater-resistant technology, specifically to a gradient-assembled solar evaporator with directional wettability, its preparation method, and its application. Background Technology

[0002] Petrochemical wastewater generated during oil extraction and refining contains abundant inorganic salts and exhibits oil-phase dispersion or emulsification. Discharge of such wastewater into the environment will severely damage aquatic systems and soil structure, thereby disrupting ecosystem stability. In industrial environments, the coexistence of various impurities promotes the formation of stable oil-in-water (O / W) emulsions, while high salinity hinders conventional separation processes, posing additional challenges. Currently, common treatment methods for O / W emulsions include high-voltage electropolymerization, ultrafiltration membrane technology, and chemical demulsification. However, the practical implementation of these technologies is often constrained by substantial operating and maintenance costs and the risk of secondary pollution.

[0003] In recent years, solar-driven interfacial evaporation (SDIE) has been widely used in seawater desalination and wastewater treatment. However, the organic matter and salts present in petrochemical wastewater hinder the efficiency of interfacial evaporation. Specifically, SDIE is constrained by several key limitations when treating oil-salt complex wastewater: (1) Salt-resistant designs exhibit limited scalability potential and neglect the balance between water transport and evaporation during salt recirculation; (2) There is relatively little research on oil-resistant methods, and existing modification methods are often characterized by complex procedures and significant environmental problems; (3) In oil-salt coexistence systems, the presence of the oil phase introduces additional transport resistance, while salt crystallization preferentially blocks microchannels, inhibiting evaporation.

[0004] Therefore, how to achieve oil and salt inhibition without affecting evaporation efficiency has become a research challenge for SDIE in the field of wastewater treatment. Summary of the Invention

[0005] This invention provides an assembled solar evaporator with a directional wettability gradient, its preparation method, and its application. This invention innovatively proposes the concept of an assembled evaporator, characterized by a wettability gradient, which can be used for the staged purification of oily and saline petrochemical wastewater. It solves the problem of performance degradation of SDIE (Synthetic Evaporator for Petrochemical Wastewater Treatment) due to oil clogging and salt accumulation when treating petrochemical wastewater.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] The present invention provides a solar evaporator with directional wettability gradient assembly, which includes, from bottom to top, an oil-blocking layer, a low-wetting water-transporting layer, and a high-wetting salt-barrier layer; the wettability relationship of the oil-blocking layer, the low-wetting water-transporting layer, and the high-wetting salt-barrier layer is as follows: the oil-blocking layer is greater than the low-wetting water-transporting layer, and the low-wetting water-transporting layer is less than the high-wetting salt-barrier layer.

[0008] This invention treats petrochemical wastewater by designing a wettability gradient, avoiding a significant decrease in evaporation rate caused by oil and salt clogging of the SDIE (Silicone Dioxide Irrigation Layer). Utilizing the wettability difference between the low-wetting water transport layer and the high-wetting salt barrier layer, water transport is precisely guided, effectively ensuring a dynamic balance between water transport and evaporation. Furthermore, before evaporation treatment, an oil barrier layer separates the oil components in the petrochemical wastewater, leaving only salt components. This separation of the complex oil-salt wastewater environment simplifies and improves the efficiency of petrochemical wastewater treatment. Simultaneously, the oil barrier layer has a higher wettability than the low-wetting water transport layer, which helps enhance oil demulsification.

[0009] Preferably, the height ratio of the low-wetting water transport layer to the high-wetting salt barrier layer is (1-3):(3-4).

[0010] Preferably, the oil-blocking layer and the low-wetting water-conveying layer are integrally formed.

[0011] Preferably, the oil-blocking layer is sodium alginate hydrogel, the low-wetting water-conducting layer is lignin-treated wood with a nano-carbon coating on its upper surface, and the high-wetting salt-blocking layer is a copper oxide rod.

[0012] Sodium alginate hydrogel, exhibiting superhydrophilicity, forms a wettability gradient with delignified wood, enhancing oil demulsification and ensuring mechanical integrity. Furthermore, copper oxide rods, characterized by ultrafast wettability response, are integrated to form another wettability gradient with the delignified wood. Positioned at the end of the water delivery channel, the vertically extending copper oxide rods expand the evaporation space, and their large sidewall contact area with air accelerates evaporation. More importantly, the copper oxide rods generate a reverse driving force for downstream water demand, promoting efficient salt recycling. Additionally, the height of the copper oxide rods is flexibly adjustable to achieve a balance between water supply and demand, effectively avoiding energy waste.

[0013] Preferably, a central hole is provided at the center of the upper surface of the low-wetting water transport layer.

[0014] Preferably, the upper surface of the low-wetting water transport layer is provided with a groove that is adapted to the size of the copper oxide rod and can be used to assemble the copper oxide rod.

[0015] Preferably, the copper oxide rods are disposed at the four vertices of the low-wetting water transport layer.

[0016] This invention provides a method for preparing a gradient-assembled solar evaporator with directional wettability, comprising:

[0017] S1. Coating the upper surface of delignified wood with nano-carbon dispersion to obtain delignified wood with nano-carbon coating on the upper surface, i.e., low wetting water transport layer.

[0018] S2. Immerse the lower surface of the low-wetting water transport layer in calcium chloride solution, then remove it and coat the lower surface of the low-wetting water transport layer with sodium alginate solution. Crosslink the sodium alginate hydrogel on the lower surface of the low-wetting water transport layer to obtain a low-wetting water transport layer with an oil-blocking layer on the lower surface.

[0019] S3. Assemble copper oxide rods on the upper surface of a low-wetting water transport layer with an oil-blocking layer on the lower surface to obtain a gradient-assembled solar evaporator with directional wettability.

[0020] Preferably, in S1, the medium for the nano-carbon dispersion is alcohol or water.

[0021] More preferably, the alcohol is methanol or ethanol.

[0022] More preferably, the coating method is spraying.

[0023] More preferably, the concentration of the nano-carbon dispersion is 0.5–3 g / L.

[0024] Preferably, in S1, the method for preparing delignified wood is as follows: the wood is soaked in a sodium chlorite solution with a pH of 4-5 at 60-100°C for at least 6 hours, and then dried to obtain delignified wood.

[0025] More preferably, the wood is balsa wood.

[0026] More preferably, the thickness of the wood is 1 to 3 cm.

[0027] More preferably, the concentration of the sodium chlorite solution is 2–5 wt%.

[0028] More preferably, the pH of the sodium chlorite solution is adjusted to 4-5 using acetic acid.

[0029] More preferably, the drying method is freeze drying.

[0030] Preferably, in step S2, the concentration of the calcium chloride solution is 400–600 mM, and the concentration of the sodium alginate solution is 4–6 wt%.

[0031] Preferably, in step S3, the copper oxide rod is prepared by immersing copper foam in a mixed solution of ammonium persulfate and sodium hydroxide, then removing and calcining it to obtain the copper oxide rod.

[0032] More preferably, the height of the copper oxide rod is 3 to 4 cm.

[0033] More preferably, the pore density of the copper foam is 80–110 ppi.

[0034] More preferably, the foamed copper is obtained by sequentially treating it with hydrochloric acid, acetone, and ethanol, followed by cleaning and drying.

[0035] More preferably, the mixed solution of ammonium persulfate and sodium hydroxide contains 0.2-0.3 M ammonium persulfate solution and 4-5 M sodium hydroxide solution.

[0036] More preferably, the soaking time is 20 to 30 minutes.

[0037] More preferably, the calcination temperature is 180–210°C, the calcination heating rate is 2–3°C / min, and the calcination time is 2–6 h.

[0038] This invention provides the application of a gradient-assembled solar evaporator with directional wettability in the treatment of complex oil and salt wastewater.

[0039] The directional wettability gradient-assembled solar evaporator provided by this invention has been proven to be effective in treating complex oil-salt wastewater. By employing a strategy of first blocking oil and then blocking salt, the oil in the complex oil-salt wastewater is removed, and the wastewater is then introduced into a low-wetting water transport layer and a high-wetting salt barrier layer. The strong hydrophilicity of the high-wetting salt barrier layer generates a reverse capillary driving force, driving the salt ions to flow back, thus achieving efficient treatment of complex oil-salt wastewater.

[0040] Preferably, the removal rate of TOC in complex oil and salt wastewater is ≥99.9%.

[0041] Therefore, the present invention has the following beneficial effects:

[0042] (1) This invention innovatively proposes the concept of an assembled evaporator, which is characterized by a wettability gradient and can be used for the graded purification of petrochemical wastewater.

[0043] (2) The present invention utilizes the synergistic effect of the mechanical strength of wood and the superhydrophilicity of hydrogel to repel oil, while the significant wettability difference between copper oxide rod and wood precisely guides the transport of water, ensuring a dynamic balance between water transport and evaporation, thereby enabling salt reflux.

[0044] (3) The present invention can further control the water supply intensity by adjusting the height of the copper oxide rod.

[0045] (4) The present invention achieves effective petrochemical wastewater treatment through the assembly of wettability gradient components. This strategy avoids the need for expensive manufacturing and energy-intensive operations and can promote the application of assembly design in the wastewater field. Attached Figure Description

[0046] Figure 1 This is a schematic diagram of the evaporator provided by the present invention.

[0047] Figure 2 This is a schematic diagram of the preparation of the evaporator provided by the present invention. a represents the assembly process, and b represents the preparation process.

[0048] Figure 3 The main performance diagrams of the evaporator are shown below. a) shows the UV-Vis-NIR spectra of M, C@M, and C@DM. b) shows the temperature changes of M, C@M, and C@DM under one sun (with the light on) and in a dark environment (with the light off). c) shows the XRD patterns of C@M and C@DM. (d) to (g) show the SEM images of M, DM, CuO, and SA, respectively. h) shows the water contact angle of M, C@M, DM, and C@DM in air. i) shows the underwater oil contact angle of M, DM, and DM / SA. j) shows the FTIR spectra of C@M and C@DM.

[0049] Figure 4 Infrared thermal images of C@M under dry conditions, in one sun (with lights on) and in a dark environment (with lights off).

[0050] Figure 5 Infrared thermograms of C@DM under dry conditions, in one sun (with lights on) and one in a dark environment (with lights off).

[0051] Figure 6 The infrared spectrum of SA hydrogel is shown.

[0052] Figure 7 The DSC curves for C@M and C@DM are shown.

[0053] Figure 8 The DSC curves are for SA hydrogel and pure water.

[0054] Figure 9 To optimize the evaporator during pure water evaporation, the following parameters are used: a) the effect of different evaporators on the evaporation rate; b) the mechanism of influence of the delignification process and CuO rods on evaporation; c) the effect of wood thickness on the evaporation rate; d) the effect of the number of CuO rods on the evaporation rate; e) the change in the mass of a large amount of water over time during evaporation at 80 and 110 ppi; f) the effect of the assembly order of C@DM and CuO on the evaporation rate; g) the mechanism of influence of the number of CuO rods in d; and h) the mechanism of influence of CF pore density in e. AER: average evaporation rate; ER: evaporation rate.

[0055] Figure 10 For salt tolerance, 'a' represents the salt concentration (3.5, 7, 10, 15 wt%) and the type of cation Na. + K + Ca 2+ Mg 2+) and types of anions (Cl - SO4 2- CO3 2- The effect of b on the evaporation rate, where b represents the salt ions (Na+) in the Bohai Sea water and the condensate after evaporation. + K + Ca 2+ Mg 2+ The concentration of ), c ​​is the 48-hour evaporation test of C@M and C@DM-4C1H in 15wt% NaCl, and d is the salt rejection mechanism of C@DM-4C1H.

[0056] Figure 11 The effect of NaCl salt concentration on the evaporation rate.

[0057] Figure 12 For cations (Na) + K + Ca 2+ Mg 2+ The effect of ) on evaporation rate.

[0058] Figure 13 For anion types (Cl) - SO4 2- CO3 2- The effect of ) on evaporation rate.

[0059] Figure 14 The change in the quality of Bohai Sea water over time during the evaporation process with and without an evaporator.

[0060] Figure 15 For oil resistance, a) shows the effect of various oil-in-water emulsions (soybean oil, diesel, n-hexane) on the evaporation rate; b) shows the effect of n-hexane concentration in water (1, 5, 10, 20 wt%) on the evaporation rate; c) shows the TOC content in PS (original oil-in-water emulsion containing 10 wt% n-hexane) and CW (condensate); insets in c show images and photomicrographs of PS and CW; d) shows a 6-cycle test of C@DM / SA-4C1H in a 1 wt% n-hexane oil-in-water emulsion; e) shows the effect of emulsion pH on the evaporation rate; f) shows the underwater oil contact angle of DM / SA in different pH environments; and g) shows the oil resistance mechanism of DM / SA.

[0061] Figure 16 Validation and outdoor testing of waste drilling fluid: a) TOC content of WDF (waste drilling fluid: a type of petrochemical wastewater) and related CW (condensate); b) 48-hour evaporation test of C@DM / SA-4C1H in waste drilling fluid; inset in b: images and photomicrographs of PS and CW; c) Na+ ion concentration after evaporation of waste drilling fluid and treated condensate. + K + Ca2+ Mg 2+ ) concentration, d is an image of the outdoor experimental setup at different times, e is detailed information on weather conditions (temperature, humidity and solar intensity) during the outdoor experiment, and f is the evaporation rate and water production rate during the outdoor experiment.

[0062] The codes in the figure are: oil barrier layer 100; low wetting water transport layer 200; nano carbon coating 210; central pore 200a; high wetting salt barrier layer 300. Detailed Implementation

[0063] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0064] In this section, copper foam (CF, 1 mm thickness) was purchased from Suzhou Keshenghe Metal Materials (Suzhou, China). Hydrochloric acid (HCl, 37%), acetone (C3H6O, 99.5%), ethanol (C2H6O, 99.5%), sodium hydroxide (NaOH, 98%), ammonium persulfate ((NH4)2S2O8), acetic acid (CH3COOH, AR), sodium alginate (C6H7NaO6, AR), and calcium chloride (CaCl2, ≥97%) were all purchased from Aladdin Chemical Co., Ltd. (Shanghai, China). Balsa wood was purchased from a timber company in Tianjin. Nano-carbon and sodium chlorite (NaClO2, AR) were purchased from Merrill Ltd. (Shanghai, China). Deionized water (DI) had a resistivity of 18.2 MΩ·cm. Bohai Sea water came from Huludao (120.81°E, 40.62°N).

[0065]

Example

[0066] Example 1

[0067] (1) Pretreatment of copper foam (CF)

[0068] The 110ppi CF with a thickness of 1mm was initially treated with hydrochloric acid, acetone and ethanol, rinsed with deionized water and dried in a vacuum environment for later use.

[0069] (2) Synthesis of CuO rods

[0070] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain CuO rods (3cm in height).

[0071] (3) Preparation of DM

[0072] A 3 cm thick layer of balsa wood was dried overnight at 105°C, and then treated with a 2 wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0073] (4) Surface modification of DM (preparation of C@DM)

[0074] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0075] (5) Formation of SA hydrogel layer

[0076] The lower surface of C@DM was first immersed in a 500mM CaCl2 solution for 5 seconds, and then a 5wt% sodium alginate (SA) solution was uniformly coated onto the CaCl2-treated area using a brush to form a cross-linked SA coating.

[0077] Assemble as follows: Precisely cut five 5×5×15mm grooves on the upper surface of the C@DM, four at the apex and one in the center (i.e., the central hole); assemble one CuO rod at each apex. The final assembled evaporator consists of three layers from top to bottom: CuO rods as a high-wetting salt barrier layer, C@DM as a low-wetting water transport layer, and SA hydrogel coating as an oil barrier layer; denoted as C@DM / SA-4C1H.

[0078] like Figure 1 As shown, the evaporator, from bottom to top, includes an oil-blocking layer 100, a low-wetting water-transporting layer 200, and a high-wetting salt-barrier layer 300. The oil-blocking layer 100 and the low-wetting water-transporting layer 200 are integrally formed. The upper surface of the low-wetting water-transporting layer 200 has grooves that are adapted to the size of the copper oxide rods for assembling the copper oxide rods. A central hole 200a is provided at the center of the upper surface of the low-wetting water-transporting layer 200, and the copper oxide rods are disposed at the four vertices of the low-wetting water-transporting layer 200.

[0079] Example 2: Wood Thickness

[0080] (1) Pretreatment of copper foam (CF)

[0081] The 110ppi CF with a thickness of 1mm was initially treated with hydrochloric acid, acetone and ethanol, rinsed with deionized water and dried in a vacuum environment for later use.

[0082] (2) Synthesis of CuO rods

[0083] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain CuO rods (3cm in height).

[0084] (3) Preparation of DM

[0085] Balsa wood (1 / 2 / 3 / 4 cm thick) was dried overnight at 105°C, then treated with 2wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0086] (4) Surface modification of DM (preparation of C@DM)

[0087] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0088] Assemble as follows: Precisely cut five 5×5×15mm grooves on the upper surface of the C@DM, four at the apex and one in the center (i.e., the central hole); assemble one CuO rod at each apex. The final assembled evaporator, from top to bottom, consists of: CuO rods as a high-wetting salt-barrier layer, and C@DM as a low-wetting water-transporting layer.

[0089] Example 3: Height of copper oxide rod

[0090] (1) Pretreatment of copper foam (CF)

[0091] The 110ppi CF with a thickness of 1mm was initially treated with hydrochloric acid, acetone and ethanol, rinsed with deionized water and dried in a vacuum environment for later use.

[0092] (2) Synthesis of CuO rods

[0093] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain 1 / 2 / 3 / 4cm CuO rods.

[0094] (3) Preparation of DM

[0095] A 3 cm thick layer of balsa wood was dried overnight at 105°C, and then treated with a 2 wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0096] (4) Surface modification of DM (preparation of C@DM)

[0097] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0098] Assemble as follows: Precisely cut five 5×5×15mm grooves on the upper surface of the C@DM, four at the apex and one in the center (i.e., the central hole); assemble one CuO rod at each apex. The final assembled evaporator, from top to bottom, consists of: CuO rods as a high-wetting salt-barrier layer, and C@DM as a low-wetting water-transporting layer.

[0099] Example 4: Copper Oxide Rod Assembly Method

[0100] (1) Pretreatment of copper foam (CF)

[0101] The 110ppi CF with a thickness of 1mm was initially treated with hydrochloric acid, acetone and ethanol, rinsed with deionized water and dried in a vacuum environment for later use.

[0102] (2) Synthesis of CuO rods

[0103] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain CuO rods (3cm).

[0104] (3) Preparation of DM

[0105] A 3 cm thick layer of balsa wood was dried overnight at 105°C, and then treated with a 2 wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0106] (4) Surface modification of DM (preparation of C@DM)

[0107] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0108] Assembly method A: Precisely cut a groove with a size of 5×5×15mm on the upper surface of C@DM, located in the center (i.e., the center hole); do not assemble CuO rods.

[0109] Assembly method B: Two grooves with dimensions of 5×5×15mm are precisely cut on the upper surface of C@DM, one at the apex and one in the center (i.e., the center hole); assemble a CuO rod at the apex.

[0110] Assembly method C: Three grooves with dimensions of 5×5×15mm are precisely cut on the upper surface of C@DM, two at the apex and one in the center (i.e., the center hole); one CuO rod is assembled at each apex.

[0111] Assembly method D: Precisely cut four grooves with dimensions of 5×5×15mm on the upper surface of C@DM, three at the apex and one in the center (i.e., the center hole); assemble one CuO rod at each apex.

[0112] Assembly method E: Five grooves with dimensions of 5×5×15mm are precisely cut on the upper surface of C@DM, four at the apex and one in the center (i.e., the center hole); one CuO rod is assembled at each apex.

[0113] Assembly method F: Five grooves with dimensions of 5×5×15mm are precisely cut on the upper surface of C@DM, four at the apex and one in the center; one CuO rod is assembled at each apex and one CuO rod is assembled in the center.

[0114] Assembly method G: Four grooves with dimensions of 5×5×15mm are precisely cut on the upper surface of C@DM, with four grooves at the vertices; one CuO rod is assembled at each vertices.

[0115] The above assembly method is described in [link to assembly instructions]. Figure 9 d.

[0116] The final assembled evaporator consists of, from top to bottom: CuO rods as a high-wetting salt-barrier layer and C@DM as a low-wetting water-transporting layer.

[0117] Example 5 CF Pore Density

[0118] (1) Pretreatment of copper foam (CF)

[0119] The 1mm thick 80 / 110ppi CF was initially treated with hydrochloric acid, acetone, and ethanol, rinsed with deionized water, and then dried in a vacuum environment for later use.

[0120] (2) Synthesis of CuO rods

[0121] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain CuO rods (3cm in height).

[0122] (3) Preparation of DM

[0123] A 3 cm thick layer of balsa wood was dried overnight at 105°C, and then treated with a 2 wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0124] (4) Surface modification of DM (preparation of C@DM)

[0125] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0126] Assemble as follows: Precisely cut five 5×5×15mm grooves on the upper surface of the delignified wood (DM), four at the apex and one in the center (i.e., the central hole); assemble one CuO rod at each apex. The final assembled evaporator, from top to bottom, consists of: CuO rods as a high-wetting salt-barrier layer, and C@DM as a low-wetting water-transporting layer.

[0127] Comparative Example 1

[0128] (1) Pretreatment of copper foam (CF)

[0129] The 110ppi CF with a thickness of 1mm was initially treated with hydrochloric acid, acetone and ethanol, rinsed with deionized water and dried in a vacuum environment for later use.

[0130] (2) Synthesis of CuO rods

[0131] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain CuO rods (3cm in height).

[0132] (3) Preparation of DM

[0133] A 3 cm thick layer of balsa wood was dried overnight at 105°C, and then treated with a 2 wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0134] (4) Surface modification of DM (preparation of C@DM)

[0135] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0136] Assemble as follows: Precisely cut five 5×5×15mm grooves on the upper surface of the C@DM, four at the apex and one in the center (i.e., the central hole); assemble one CuO rod at each apex. The final assembled evaporator, from top to bottom, is as follows: CuO rod as a high-wetting salt barrier layer, C@DM as a low-wetting water transport layer; C@DM-4C1H.

[0137] Comparative Example 2: Changes in Wetting Gradient Direction

[0138] (1) Pretreatment of copper foam (CF)

[0139] The 110ppi CF with a thickness of 1mm was initially treated with hydrochloric acid, acetone and ethanol, rinsed with deionized water and dried in a vacuum environment for later use.

[0140] (2) Synthesis of CuO rods

[0141] Pretreated CF with a cross-section of 5×5mm was taken out and immersed in 5M NaOH solution and 0.26M (NH4)2S2O8 solution for 30min. The treated sample was rinsed three times with ethanol and deionized water, then dried in an oven at 80℃ for 8h, and then placed in a tube furnace and heated in air atmosphere (200℃, heating rate: 2℃ / min) for 2h to finally obtain CuO rods (3cm in height).

[0142] (3) Preparation of DM

[0143] A 3 cm thick layer of balsa wood was dried overnight at 105°C, and then treated with a 2 wt% NaClO2 solution (pH adjusted to 4.6 with CH3COOH) at 80°C for 6 hours to remove lignin. The lignin-freezed wood was then freeze-dried to obtain delignified wood, denoted as DM.

[0144] (4) Surface modification of DM (preparation of C@DM)

[0145] A nano-carbon (1 g / L) ethanol dispersion was sprayed and uniformly coated onto the upper surface of DM to prepare C@DM.

[0146] Assemble as follows: precisely cut five 5×5×15mm grooves on the upper surface of C@DM, four at the apex and one in the center (i.e., the center hole); assemble one CuO rod at each apex.

[0147] Assembled to obtain:

[0148] Evaporator A consists of, from top to bottom: CuO rod, C@DM; denoted as C@DM / -4C1H.

[0149] Evaporator B, from top to bottom, consists of: C@DM and CuO rod; denoted as RE-C@DM-4C1H.

[0150] The above assembly method is described in [link to assembly instructions]. Figure 9 f.

[0151] Comparative Example 3

[0152] Balsa wood was dried overnight at 105°C to obtain wood, denoted as M. An ethanol dispersion of nano-carbon (1 g / L) was sprayed onto the upper surface of M to prepare C@M.

[0153] [Performance Testing]

[0154] Solar Evaporation Experiment: The indoor solar evaporation experiment was conducted in a laboratory environment (ambient temperature approximately 30℃, humidity approximately 30%). A xenon lamp (PLS-SXE300+, Perfect Light) with an AM1.5G filter was used to simulate sunlight. A light power meter (CEL-FZ-A, Aulight) was used to detect light intensity. Moisture loss during the evaporation process was continuously monitored by an electronic balance, and temperature changes were analyzed by an infrared camera (DT9897, CEM). Meteorological conditions during the outdoor experiment were recorded by a meteorological monitoring station (FST100-QXZ-01).

[0155] The subject of the single evaporation experiment was seawater from the Bohai Sea.

[0156] The object to be treated in oil-salt composite processes is waste drilling mud.

[0157] 1. Photothermal properties, morphology, and hydrophilicity

[0158] Figure 3 (a) shows the light absorption properties of M, C@M, and C@DM. Compared to M, both C@M and C@DM exhibit particularly strong absorption. Notably, the delignification process in C@DM has the least impact on its light absorption performance, with an average absorbance of 91.28% calculated by integration. Figure 3 (b) shows the temperature rise curves of different materials under one solar irradiation. Notably, C@DM reached a temperature of 63.8 °C in just 1 minute, which is 174.14% higher than M. Furthermore, C@DM reached a peak temperature of 77.3 °C, which is sufficient to provide ample energy for evaporation. Figure 4 and Figure 5 In contrast, the higher surface temperature only occurs in the top layer, with a significant thermal gradient along the cross-section, highlighting its superior thermal insulation performance as a photothermal substrate.

[0159] Figure 3 (c) shows the XRD diffraction of C@M and C@DM. Delignification did not destroy the original crystal structure, but slightly reduced some of the broad amorphous diffraction signals. In addition, the intensity of the diffraction peaks corresponding to the cellulose crystal planes was significantly enhanced, such as (101), (002) and (040). Figure 3 (d)–(g) show the morphology of the evaporator. Compared to M, DM exhibits a significantly increased number of channels, enhancing moisture transport. The surface of the CuO rod is covered with numerous micro / nanospins, further elucidating the strong capillary action. The SA hydrogel is primarily composed of interconnected hexahedral aggregates with tightly distributed and relatively small pores, contributing to its effective oil resistance by inhibiting the entry of oil molecules.

[0160] Figure 3 (h) illustrates the evolution of hydrophilicity. The transition from M to C@M resulted in a decrease in hydrophilicity; C@M even maintained a water contact angle of 27.48° after 10 seconds of wetting, attributed to the inherent hydrophobicity of nano-carbon. Conversely, modification from M to DM enhanced hydrophilicity, halving the wetting time from 0.1 seconds to 0.05 seconds. Introducing nano-carbon into C@DM resulted in a moderate decrease in hydrophilicity, increasing the wetting time from 0.05 seconds to 0.35 seconds. The controlled decrease in surface hydrophilicity effectively balanced photothermal management and water transport, and was therefore acceptable. The oil repellency of the evaporator was quantitatively evaluated by underwater oil contact angle measurements. Figure 3 (i)). After delignification, it moderately increased from 107.33° to 113.40°. Subsequently, with the addition of SA hydrogel, this parameter increased significantly to 143.69°, demonstrating its superior ability to separate oil / water emulsions efficiently.

[0161] FTIR spectra of wood and SA hydrogel as follows Figure 3 (j) and Figure 6 As shown. Compared to C@M, C@DM at 3350cm -1 An enhanced OH stretching vibration signal was observed in the vicinity, attributed to the exposure of hydroxyl groups in cellulose and hemicellulose after delignification. 2900cm -1 The enhanced CH stretching vibrations at this location originate from abundant aliphatic moieties, confirming a complete delignification process. SA spectra reveal characteristic structural features at 3320 cm⁻¹. -1 The broadband at 1600 cm⁻¹ originates from intermolecular and intramolecular hydrogen bonds. -1 The nearby absorption confirmed the presence of the carboxylic acid group (COO-), which is consistent with the superhydrophilicity. Figure 7 and Figure 8 The state of water in the evaporator was elucidated using DSC analysis. Due to the inherent microchannels of natural wood, the enthalpy of vaporization of pressurized water was approximately 1571 kJ / kg. After delignification, this enthalpy decreased significantly by 42.97% to 896 kJ / kg, indicating a significant reduction in evaporation resistance at the microscopic level. These results demonstrate that DM and SA significantly reduce the enthalpy of water during evaporation.

[0162] 2. Optimization of evaporators in pure water evaporation

[0163] 2.1 Delignification effect and introduction of CuO rod

[0164] like Figure 9 As shown in (a), delignification alone reduced the evaporation rate under one sun from 1.23 kg·m³. -2 ·h -1 Slightly reduced to 1.20 kg·m -2 ·h -1 To address this problem, increasing the evaporation rate should be a priority. The inventors have unprecedentedly assembled balsa wood with CuO rods possessing excellent evaporation surfaces, abandoning the traditional monolithic design and instead utilizing the sidewall evaporation effect to significantly improve overall performance. As a result, the evaporation rate increases to 2.08 kg·m³. -2 ·h -1 This represents an increase of 69.11%. The combination of DM and CuO simultaneously improves both water supply and evaporation demand, achieving a better balance and providing 2.29 kg·m³. -2 ·h -1The evaporation rate increased by 85.85% compared to the original configuration. Compared to traditional wood-based evaporators, delignification increases the porosity of the wood, thereby promoting water transport. Integrating CuO rods into the DM enhances the evaporation threshold of traditional wood-based evaporators through CuO's superior omnidirectional evaporation capabilities, narrowing the gap between transport and evaporation. The synergistic integration of delignification (enhanced water transport capacity) and CuO rods (improved evaporation performance) amplifies both the supply and demand aspects of the evaporation process, avoiding excessive energy loss while ensuring excellent evaporation efficiency. Figure 9 (b)).

[0165] 2.2 Influence of CuO rod height

[0166] The height of the CuO rod is used to regulate the balance between evaporation and water transport. As shown in Table 1, the evaporation rate increases accordingly from 1.20 kg·m³ as the CuO rod height increases from 0 to 3 cm. -2 ·h -1 Increased to 1.37 kg·m -2 ·h -1 1.69 kg·m -2 ·h -1 and 2.29 kg·m -2 ·h -1 This indicates that the CuO rod effectively utilizes the water transported through the wood to enhance evaporation. However, when the height is further increased to 4 cm, the improvement in evaporation rate is not significant. Therefore, a height of 3 cm is the optimal choice.

[0167] Table 1. Effect of copper oxide rod height on evaporation rate

[0168]

[0169] 2.3 Effect of wood thickness

[0170] The thickness of the wood also affects its evaporation performance, as the porous sidewalls allow some vapor to escape. For example... Figure 9 As shown in (c), when the wood thickness increases from 1 cm to 3 cm, the evaporation rate increases from 2.13 kg·m³. -2 ·h -1 It rose to 2.29 kg·m -2 ·h -1 This indicates that the sidewall contributes to the overall evaporation process. However, when it is further increased to 4 cm, the evaporation rate decreases slightly to 2.23 kg·m³. -2 ·h -1 This reduction may be due to the increased water migration distance, disrupting the balance between water supply and evaporation. Therefore, a 3cm thick layer of wood was selected for subsequent experiments.

[0171] Table 2 Effect of wood thickness on evaporation rate

[0172]

[0173] 2.4 Effect of eliminating evaporation dead zone

[0174] Minimizing the number of CuO rods while maintaining effective evaporation is a feasible strategy to reduce material costs and improve practical feasibility in petrochemical wastewater scenarios. For example... Figure 9 As shown in (d), when five CuO rods are uniformly assembled on the surface of wood, the evaporation rate is only 1.93 kg·m⁻². -2 ·h -1 Interestingly, when the central CuO rod was removed, leaving four rods and a central hole was introduced, the evaporation rate increased by 37.80%, reaching 2.66 kg·m³. -2 ·h -1 Further continuous removal of the outer rods resulted in a gradual decrease in the evaporation rate, which can be attributed to a reduction in the omnidirectional evaporation promoted by the surrounding CuO rods. The evaporation rate results obtained from the evaporator in Assembly Method G of Example 4 further highlight the protrusion of the central hole. When four CuO rods were inserted around the central hole, the presence of the central hole significantly enhanced evaporation, increasing the evaporation rate by 16.4% from the initial 2.29 kg·m³. -2 ·h -1 Increased to 2.6 kg·m -2 ·h -1 Furthermore, it achieves a 112.20% improvement compared to traditional wooden evaporators. Figure 9 (g) illustrates the effect of the central orifice on evaporation performance. Due to the limited air convection directly above a large evaporation center, it often becomes a bottleneck for steam diffusion, hindering effective steam diffusion (dead zone). Removing this section can promote more efficient steam release and facilitate sustainable high-performance evaporation.

[0175] Table 3. Effect of Assembly Method on Evaporation Rate

[0176]

[0177] 2.5 Effect of CF pore density

[0178] Figure 9 (e) highlights the effect of CF pore density (measured in ppi) on the evaporation process. As it increases from 80 to 110, the evaporation rate increases from 2.39 kg·m³. -2 ·h -1 Increased to 2.66 kg·m -2 ·h -1 This is related to Figure 9 (e) insertion Figure 1Therefore, under the same solar radiation, 110ppi carbon fiber has a lower surface temperature. Figure 9 (h) further explains the mechanism by which pore density affects evaporation. Given the inherently high thermal conductivity of carbon fibers, their surface temperature may drop below ambient temperature during evaporation. Therefore, in addition to utilizing solar radiation, the system can also obtain supplementary energy from the surrounding environment. The lower surface temperature of 110 ppi CF allows for more efficient absorption of ambient energy, promoting evaporation.

[0179] Table 4. Effect of CF pore density on evaporation rate

[0180]

[0181] 2.6 Influence of changes in the direction of wetting gradient

[0182] Figure 9 (f) illustrates the differences in evaporation performance resulting from different assembly configurations of wood and CuO rods. When CuO is in the upper layer, C@DM-4C1H is formed, and the evaporation rate reaches 2.66 kg·m⁻¹. -2 ·h -1 Conversely, when they are reversed, the evaporation rate decreases by 34.72% to 1.74 kg·m³. -2 ·h -1 Considering the data in Table 5, which shows that the CuO rod exhibits a water transport rate of 2.294 cm / s, exceeding the height of DM by 97.62%, placing CuO at the end of the water transport channel utilizes its stronger capillary effect to continuously drive the water supply. Conversely, when the structure is inverted, it cannot effectively accommodate incoming water, nor can it utilize the resulting capillary gradient to enhance transport.

[0183] Table 5. Water transport rates of DM and CuO rods

[0184]

[0185] 3. Evaluation of desalination performance

[0186] 3.1 Effects of Salinity and Ion Species

[0187] The effect of salt ion concentration on the performance of C@DM-4C1H is as follows: Figure 10 As shown in (a), taking NaCl as an example, when its concentration increases from 3.5 wt% (average salinity of seawater) to 15 wt% (high salinity), the evaporation rate under one sun shows a slight decrease, from a maximum of 2.32 kg·m³. -2 ·h -1 It decreased to 2.05 kg·m -2 ·h -1This corresponds to a reduction of 11.61%. This reduction is considered acceptable because the saturated vapor pressure of a solution typically decreases with increasing solute concentration. Notably, even with an increase in salinity of approximately 300%, the evaporation rate only decreased by about 10%, indicating a strong adaptability to salinity changes.

[0188] The corresponding result reproducibility is as follows Figures 11-13 As shown. Except for Na + and Cl - In addition, seawater and wastewater usually contain potassium. + Ca 2+ Mg 2+ SO4 2- and CO3 2- Other substances, such as cations and anions, are also studied. However, the effects of these ions on the evaporation process are not yet fully understood. The effects of various cations and anions on evaporator performance were systematically investigated. Figure 10 (a)). Regarding the effect of cations, under the same experimental conditions, a 15 wt% KCl solution exhibited the highest evaporation rate, reaching 2.13 kg·m⁻². -2 ·h -1 The order of evaporation is NaCl, MgCl2, and CaCl2. The evaporation rate largely depends on the ability of water molecules from the liquid surface to escape into the gas phase, a process directly influenced by the equilibrium vapor pressure. Compared to divalent salts, KCl and NaCl experience relatively smaller vapor pressure drops due to weaker colligative effects, while CaCl2... 2+ and Mg 2+ Its strong hydration tendency further suppresses vapor pressure. As for the anion CO3... 2- The evaporation rate of 15 wt% Na₂CO₃ was the lowest, at only 1.99 kg·m³. -2 ·h -1 This can be attributed to its relationship with CO3. 2- Related significant colligative effects and strong hydration

[0189] 3.2 Seawater Verification

[0190] Validation using actual seawater is crucial for demonstrating the practical applicability of the evaporator. Bohai Sea water is used to evaluate performance under complex natural environments. Figure 14 Under one sun, the evaporation rate reaches as high as 2.59 kg·m³. -2 ·h -1 Even under the challenging conditions of the Bohai Sea, it was 47 times higher than the control group. Furthermore, the generated condensate was collected and analyzed. Figure 10(b) Compared to the original seawater, the concentrations of the four representative cations were reduced by more than two orders of magnitude, successfully meeting the World Health Organization's drinking water standards. These results validate the feasibility and effectiveness of the seawater desalination evaporator.

[0191] 3.3 Stability under long-term evaporation

[0192] like Figure 10 As shown in (c), the evaporation performance of different evaporators in 15 wt% NaCl solution was studied for more than 48 hours. C@DM-4C1H exhibited a relatively stable evaporation rate throughout the 48 hours, maintaining 2.12 kg·m³. -2 ·h -1 The average evaporation rate was [missing information], and no visible salt buildup was observed on the surface after prolonged operation. In contrast, C@M exhibited a gradual decline in performance, with the evaporation rate decreasing from 0.71 to 0.49 kg·m³. -2 ·h -1 The decrease was 30.99%. Furthermore, significant salt crystallization was observed on its surface after 48 hours of testing, highlighting its limited durability under high salinity conditions.

[0193] 3.4 Salt rejection mechanism

[0194] The specific salt resistance mechanism of C@DM-4C1H, such as Figure 10 As shown in (d), in the monolithic evaporator C@M, salt ions tend to rise with the upward water flow. Under continuous evaporation, the localized accumulation of salt on the photothermal surface can block the water transport path, hindering light absorption and vapor release. In contrast, C@DM-4C1H effectively circumvents this problem by introducing CuO rods, which disrupt the single water transport path and form asymmetric channels. Nano-CuO exhibits excellent hydrophilicity, providing a strong water demand at the transport endpoint. This constant water inflow has a flushing effect on salt ions, promoting their reflux rather than allowing them to accumulate at the photothermal interface or block transport paths.

[0195] 4. Evaluation of oil resistance

[0196] 4.1 Effects of different oil-in-water emulsions

[0197] Soybean oil, diesel oil, and n-hexane were selected as three representative oils to study the oil resistance properties of emulsified C@DM / SA-4C1H. Figure 15 (a)). Compared with blank evaporation, C@DM / SA-4C1H achieved evaporation rates of 52, 44, and 33 times in three corresponding emulsion systems, demonstrating that the evaporator can effectively overcome mass transfer resistance and achieve efficient evaporation even in the presence of oil-water emulsions.

[0198] Table 6 shows the treatment effects of C@DM-4C1H and C@DM / SA-4C1H evaporators on 10% oil-containing emulsions (n-hexane) under sunlight. Observations indicate that the SA hydrogel layer helps block oil in the oil-in-water emulsion, making the wastewater composition after oil removal simpler, thereby helping to increase the evaporation rate.

[0199] Table 6. Effect of SA on the oil and salt inhibition effect of the evaporator

[0200]

[0201] 4.2 Effect of oil concentration

[0202] Figure 15 (b) illustrates the effect of oil concentration in the emulsion on evaporation performance. Taking highly volatile n-hexane as an example, the evaporation rate under one sun gradually decreases as its concentration increases from 1 wt% to 5 wt%, 10 wt%, and 20 wt%. Even at a high oil content of 20 wt%, the evaporation rate still reaches 2.09 kg·m³. -2 ·h -1 As oil content increases, the observed decrease in evaporation performance is inevitable, primarily due to the increased resistance associated with the microscopic demulsification process. Densely distributed oil droplets tend to form tightly packed structures, which enhances mechanical resistance and hinders droplet migration and coalescence. For the evaporation of emulsions, especially those containing volatile oil phases, process feasibility assessments must consider not only evaporation performance but also the content of organic compounds in the condensate. Figure 15 (c) Total organic carbon (TOC) data for the original oil-in-water emulsion containing 10 wt% n-hexane and the corresponding treated condensate. Compared to the original oil-in-water emulsion, the TOC content in the condensate was reduced by nearly three orders of magnitude, and the condensate appeared clear and transparent. Microscopic analysis further confirmed that the original oil-in-water emulsion treated with C@DM / SA-4C1H had transformed into clear condensate without any oil content, indicating that C@DM / SA-4C1H can completely block oil.

[0203] 4.3 Cyclic Testing

[0204] SA hydrogels are typically brittle, exhibit poor tensile strength, and are prone to mechanical failure. Figure 15 (d) shows the evaporation performance of C@DM / SA-4C1H during multiple cycles in a 10 wt% oil-containing emulsion (n-hexane). After six consecutive cycles, the evaporation rate remained stable at approximately 2.50 kg·m³. -2 ·h -1 There was no significant decrease, indicating that attaching SA hydrogel as a membrane to wood effectively enhances its structural integrity, reduces the frequency of damage, and prevents a decline in evaporation performance due to material failure.

[0205] 4.4 Effect of pH

[0206] The pH range of petrochemical wastewater is typically between 5 and 9.37. To investigate the effect of pH changes on the system's oil resistance, the evaporation behavior of a 10 wt% oil-containing emulsion (n-hexane) was examined under three representative pH conditions (5, 7, and 9). Figure 15 (e)). When the pH value increases from 5 to 7, the evaporation rate increases from 2.32 kg·m³. -2 ·h -1 It decreased slightly to 2.23 kg·m -2 ·h -1 When the pH value was further increased to 9, the evaporation rate increased slightly to 2.24 kg·m³. -2 ·h -1 In general, the effect of pH changes on emulsion evaporation performance is negligible, a fact further confirmed by changes in the underwater oil contact angle. Figure 15 (f) This indicates that the SA hydrogel maintained its function within the tested pH range, demonstrating a degree of adaptability to the variable conditions commonly encountered in the petrochemical wastewater field.

[0207] 4.5 Oil Resistance Mechanism

[0208] Figure 15 (g) illustrates the oil-resistant mechanism of C@DM / SA-4C1H obtained through gradient assembly. Traditional monolithic wood evaporators cannot effectively separate oil and water, often resulting in partial oil evaporation during the evaporation process. While pure hydrogels can provide underwater superhydrophilicity and oleophobicity, their inherent fragility makes them prone to mechanical failure, thus compromising long-term operational stability. In this invention, the evaporator design combines the mechanical strength of wood with the oil-repellent properties of SA hydrogels. The thin hydrogel layer at the bottom enables emulsion demulsification, capturing coalesced oil droplets at the interface. Simultaneously, water molecules rapidly permeate the hydrogel and are transported upwards through microchannels in the wood. Furthermore, the hydrogel layer extends along the side portion of the wood, serving a dual purpose: preventing lateral penetration of oil that could disrupt the directional evaporation process, and enhancing the adhesion between the hydrogel and the wood.

[0209] 4.6 Verification using real petrochemical wastewater

[0210] Furthermore, C@DM / SA-4C1H was used to treat typical petrochemical wastewater—waste drilling fluid (WDF). For example... Figure 16 As shown in (a), the treated condensate (CW) exhibits a TOC removal efficiency of up to 99.94% compared to the original WDF. Figure 16(b) shows the results of a 48-hour evaporation experiment using C@DM / SA-4C1H containing WDF. Throughout the long-term operation, the evaporation rate remained stable at 2.41 kg·m³. -2 ·h -1 The illustration shows a clear transformation from the initial brownish-yellow WDF to transparent condensate, visually confirming the purification process. Microscopic imaging further demonstrates the high cleanliness of the condensate. Ion concentrations in both WDF and CW are also shown. Figure 16 (c) shows that four common salt ions were removed with efficiencies ranging from 97.65% to 99.56%, demonstrating excellent desalination capabilities.

[0211] 4.7 Outdoor Assessment

[0212] Under outdoor conditions, the C@DM / SA-4C1H system is used to treat petrochemical wastewater. Figure 16 (e) and Table 7 show the weather conditions recorded during a week-long outdoor experiment conducted daily from 9:00 to 17:00, with daily average temperature, humidity, and solar irradiance at 27.65 °C, 38.08%, and 60.94 mW·cm⁻¹, respectively. -2 Measurements were taken. The experiment was conducted at the Beiyangyuan Campus of Tianjin University in Tianjin, China. Operation began at 9:00 AM, and within 30 minutes, a large amount of water vapor was observed to condense on the inclined condenser mounted above the evaporator. Figure 16 (d)). Figure 16 (f) The average daily evaporation rate and water yield over the week were summarized, reaching 1.61 kg·m³. -2 ·h -1 and 10.62 kg·m -2 ·day -1 .

[0213] Table 7 Weather conditions during outdoor testing

[0214]

[0215] Table 8. Average annual solar radiation in typical cities (mW·cm²) -2 (Taking 2021 as an example)

[0216]

[0217] Table 9. Estimated daily water production in typical global cities.

[0218]

Claims

1. A gradient-assembly solar evaporator with directional wettability, characterized in that, From bottom to top, it includes an oil-blocking layer, a low-wetting water-transporting layer, and a high-wetting salt-barrier layer; the wettability relationship of the oil-blocking layer, the low-wetting water-transporting layer, and the high-wetting salt-barrier layer is as follows: the oil-blocking layer is greater than the low-wetting water-transporting layer, and the low-wetting water-transporting layer is less than the high-wetting salt-barrier layer; the oil-blocking layer is sodium alginate hydrogel, the low-wetting water-transporting layer is lignin-treated wood with a nano-carbon coating on its upper surface, and the high-wetting salt-barrier layer is a copper oxide rod.

2. The gradient-assembly solar evaporator with directional wettability as described in claim 1, characterized in that, The thickness ratio of the low-wetting water-conveying layer to the high-wetting salt-barrier layer is (1~3):(3~4).

3. The gradient-assembly solar evaporator with directional wettability as described in claim 1, characterized in that, The oil-blocking layer and the low-wetting water-conducting layer are integrally formed.

4. The gradient-assembly solar evaporator with directional wettability as described in claim 2 or 3, characterized in that, A central hole is provided at the very center of the upper surface of the low-wetting water transport layer.

5. The gradient-assembly solar evaporator with directional wettability as described in claim 2 or 3, characterized in that, The upper surface of the low-wetting water transport layer is provided with grooves that are adapted to the size of the copper oxide rods and can be used to assemble the copper oxide rods.

6. The gradient-assembly solar evaporator with directional wettability as described in claim 2 or 3, characterized in that, The copper oxide rods are positioned at the four vertices of the low-wetting water transport layer.

7. A method for preparing a gradient-assembly solar evaporator with directional wettability as described in any one of claims 1 to 6, characterized in that, include: S1. Coating the upper surface of delignified wood with nano-carbon dispersion to obtain delignified wood with nano-carbon coating on the upper surface, i.e., low wetting water transport layer. S2. Immerse the lower surface of the low-wetting water transport layer in calcium chloride solution, then remove it and coat the lower surface of the low-wetting water transport layer with sodium alginate solution. Crosslink the sodium alginate hydrogel on the lower surface of the low-wetting water transport layer to obtain a low-wetting water transport layer with an oil-blocking layer on the lower surface. S3. Assemble copper oxide rods on the upper surface of a low-wetting water transport layer with an oil-blocking layer on the lower surface to obtain a gradient-assembled solar evaporator with directional wettability.

8. The preparation method according to claim 7, characterized in that, In S1, the concentration of the nano-carbon dispersion is 0.5~3g / L.

9. The preparation method according to claim 7, characterized in that, In S1, the medium for the nano-carbon dispersion is alcohol or water.

10. The preparation method according to claim 9, characterized in that, The alcohol is methanol or ethanol.

11. The preparation method according to claim 7, characterized in that, In S1, the coating method is spraying.

12. The preparation method according to claim 7, characterized in that, In S1, the method for preparing delignified wood is as follows: the wood is soaked in a sodium chlorite solution with a pH of 4-5 at 60-100°C for at least 6 hours, and then dried to obtain delignified wood.

13. The preparation method according to claim 12, characterized in that, The wood is balsa wood.

14. The preparation method according to claim 12, characterized in that, The thickness of the wood is 1 to 3 cm.

15. The preparation method according to claim 12, characterized in that, The concentration of the sodium chlorite solution is 2-5 wt%.

16. The preparation method according to claim 12, characterized in that, Adjust the pH of the sodium chlorite solution to 4-5 using acetic acid.

17. The preparation method according to claim 12, characterized in that, The drying method is freeze drying.

18. The preparation method according to claim 7, characterized in that, In S2, the concentration of calcium chloride solution is 400-600 mM, and the concentration of sodium alginate solution is 4-6 wt%.

19. The preparation method according to claim 7, characterized in that, In S3, the method for preparing copper oxide rods is as follows: copper foam is immersed in a mixed solution of ammonium persulfate and sodium hydroxide, then removed and calcined to obtain copper oxide rods.

20. The preparation method according to claim 19, characterized in that, The height of the copper oxide rod is 3~4 cm.

21. The preparation method according to claim 19, characterized in that, The pore density of copper foam is 80~110 ppi.

22. The preparation method according to claim 19, characterized in that, Copper foam is obtained by sequentially treating it with hydrochloric acid, acetone, and ethanol, followed by cleaning and drying.

23. The preparation method according to claim 19, characterized in that, The mixed solution of ammonium persulfate and sodium hydroxide contains 0.2-0.3 M ammonium persulfate solution and 4-5 M sodium hydroxide solution.

24. The preparation method according to claim 19, characterized in that, Soaking time is 20-30 minutes.

25. The preparation method according to claim 19, characterized in that, The calcination temperature is 180~210℃, the heating rate is 2~3℃ / min, and the calcination time is 2~6 h.

26. The application of the directional wettability gradient-assembled solar evaporator as described in any one of claims 1 to 6, or the directional wettability gradient-assembled solar evaporator prepared by the preparation method as described in any one of claims 7 to 25, in the treatment of complex oil and salt wastewater.

27. The application as described in claim 26, characterized in that, The removal rate of TOC in complex oil and salt wastewater is ≥99.9%.

Citation Information

Patent Citations

  • Photothermal conversion film, preparation method thereof and double-layer evaporation structure for solar steam generation

    CN110726262A

  • Preparation method of photothermal conversion porous structure and solar evaporation device

    CN113860354A