Electrode grid line, preparation method thereof and conductive paste
By using a seed layer and base metal layer stacking process and setting contact feet to compensate for printing deviations, the problems of high silver consumption and high overlap accuracy requirements in photovoltaic cells are solved, thereby reducing silver consumption and improving electrical conductivity.
Patent Information
- Application Number
- CN202511473113.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-15
- Publication Date
- 2026-01-09
AI Technical Summary
In existing photovoltaic cells, the high precision required for the overlap between the main grid and the fine grid results in high silver consumption and unsatisfactory product yield. Current methods to reduce silver consumption by decreasing the width of the fine grid lines have limited effectiveness.
A seed layer and base metal layer stacking process is adopted. Contact feet are set in the fine gate of the seed layer and the fine gate of the base metal layer. The base metal accounts for more than 68% of the conductive phase of the base metal layer. The width of the contact feet in the fine gate linewidth direction is greater than the fine gate linewidth. The contact feet compensate for printing accuracy deviation and reduce the printing accuracy requirements.
It effectively reduces the silver consumption of the electrode grid line by about 87%, improves electrical conductivity and product yield, and achieves efficient longitudinal current conduction.
Smart Images

Figure CN121310708A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of photovoltaic cell technology, and in particular to an electrode grid line, its preparation method, and a conductive paste. Background Technology
[0002] In photovoltaic cells, the main grid and the fine grid form a hierarchical current collection network. The fine grid, typically 30-50 μm wide, serves as a high-density distributed microelectrode that directly covers the light-receiving surface of the cell to collect photogenerated carriers. The main grid, typically 0.8-1.8 mm wide, is arranged perpendicular to the fine grid and collects the fine grid current through the overlap point, leading to the external circuit. The two work together to achieve the functional coupling of micro-collection and macro-conduction. The overlap accuracy and contact resistance directly determine the series loss of the cell.
[0003] The main busbar and fine grid are typically printed using conductive silver paste. The linewidth and number of the main busbar and fine grid are important factors affecting the silver consumption of photovoltaic cells, and reducing silver consumption is a crucial way to reduce the cost of photovoltaic cells. For example, when the number of main busbars in p-type cells is increased from 9BB to 11BB and 16BB, the silver consumption on the front side is reduced to about 65mg / cell, and the silver consumption on the back side is about 26mg / cell; the average silver consumption on both sides of n-type TOPCon cells is about 80mg / cell; and the silver consumption on both sides of heterojunction cells is about 110mg / cell. On the one hand, both the main busbar and fine grid have corresponding height requirements, and the effect of reducing silver consumption by reducing the linewidth is limited; on the other hand, the overlapping of the main busbar and fine grid requires positioning printing through edge gripping and mark point gripping, which requires high precision (±5μm) and the product yield is not ideal. Summary of the Invention
[0004] To address the aforementioned issues and improve yield by reducing both silver consumption and printing precision requirements, a first aspect of this application provides an electrode gate line comprising a seed layer printed on a silicon wafer surface and a base metal layer superimposed on the seed layer. The base metal layer has a base metal content greater than 68% in its conductive phase. The seed layer includes a main gate and a seed layer fine gate. The base metal layer includes base metal layer fine gates that are electrically connected to the seed layer fine gates one-to-one. At least one of the seed layer fine gates and the base metal layer fine gates is further provided with a plurality of contact feet. The contact feet are spaced apart along the length direction of their corresponding fine gates, and the width of each contact foot in the linewidth direction of its corresponding fine gate is greater than the linewidth of its corresponding fine gate.
[0005] In some alternative implementations, the contact feet are evenly distributed between every two adjacent main gates, and the shape of the contact feet is one or more of rhombus, square, ellipse and linear.
[0006] In some optional embodiments, the width of the contact foot in the linewidth direction of its respective fine grid is 30-100 μm, and the length of the contact foot in the length direction of its respective fine grid is 3-30 μm.
[0007] The second aspect of this application provides a method for preparing electrode grid lines as described in any of the preceding claims, comprising the following steps: S1: preparing a seed layer screen and a base metal layer screen according to the number and linewidth information of the main grid and fine grid of the electrode grid lines, wherein the seed layer screen is a screen combining the main grid pattern and the fine grid pattern, and the base metal layer screen only contains the fine grid pattern, and at least one of the seed layer screen and the base metal layer screen has a plurality of contact pin patterns on the fine grid pattern, the contact pin patterns being spaced apart along the length direction of the fine grid pattern, and the width of the contact pin pattern being greater than the width of the fine grid pattern in which it is located; S2: screen printing a seed layer of the back electrode on the back side of a silicon wafer using the seed layer screen and conductive paste, with a printing pressure of 50 N / cm² and a printing speed of 500 mm / s, followed by drying and heat treatment; S3: screen printing a base metal layer superimposed on the seed layer in step S2 using the base metal layer screen and conductive paste, with a printing pressure of 50 N / cm² and a printing speed of 500 mm / s. mm / s, dry and heat-treated to obtain the electrode grid lines of the back electrode; S4: Referring to steps S2 and S3, screen print the seed layer and the base metal layer on the front side of the silicon wafer to obtain the electrode grid lines of the front electrode.
[0008] To reduce silver consumption, a third aspect of this application provides a conductive paste for printing electrode grid lines as described in any of the above claims or electrode grid lines prepared by the above-described electrode grid line preparation method. The conductive paste includes a seed layer paste for preparing the seed layer and a base metal layer paste for preparing the base metal layer. The conductive phase of the seed layer paste is silver powder, and the mass percentage of the silver powder in the seed layer paste is 20-80 wt%. The conductive phase of the base metal layer paste is base metal powder or a mixture of base metal powder and silver powder, and the mass percentage of the base metal powder in the base metal layer paste is 60-90 wt%. The mass percentage of the silver powder in the base metal layer paste is 0-30 wt%. The fineness of the seed layer paste is below 5 μm and the viscosity is 30-80 Pa·s. The fineness of the base metal layer paste is below 10 μm and the viscosity is 50-100 Pa·s.
[0009] In some optional embodiments, the silver powder is spherical, flake-shaped, or irregularly shaped, with a D50 particle size ranging from 1.2 to 1.8 μm and a tap density of 5.0 to 7.0 g / cm³. 3 Its specific surface area is 0.5-0.7 m². 2 / g, wherein the base metal powder is one or more selected from nickel powder, copper powder, tungsten powder, chromium powder, molybdenum powder, nickel-based alloy powder, copper-based alloy powder, silver-coated nickel powder, and silver-coated copper powder, with a D50 particle size range of 0.3-10μm and a tap density of 5.0-7.0g / cm³. 3 Its specific surface area is 0.5-2.5 m². 2 / g.
[0010] In some optional embodiments, the seed layer slurry further includes the following components by weight percentage: 0.5-6 wt% glass powder and 15-75 wt% organic carrier; the glass powder used in the seed layer slurry includes at least four of PbO, TeO2, Bi2O3, SiO2, Al2O3, ZnO, and WO3.
[0011] In some alternative embodiments, the glass powder used in the seed layer slurry comprises the following components by weight percentage: 40wt% PbO, 2.0wt% SiO2, 30wt% TeO2, 20wt% Bi2O3, 3.0wt% ZnO and 5.0wt% WO3.
[0012] In some optional embodiments, the base metal layer slurry further includes the following components by mass percentage: 0-3 wt% glass powder, 5-15 wt% organic carrier, wherein the glass powder used in the base metal layer slurry includes at least five of the following: PbO, TeO2, Bi2O3, SiO2, Al2O3, ZnO, Cu2O, MnO, TiO2, and B2O3.
[0013] In some alternative embodiments, the glass powder used in the base metal layer slurry comprises the following components by weight percentage: 10wt% PbO, 40wt% SiO2, 2.0wt% TeO2, 5.0wt% Bi2O3, 3.0wt% ZnO, 4.0wt% Al2O3, 20wt% Cu2O, 5.0wt% TiO2, 10wt% MnO, and 1.0wt% B2O3.
[0014] In some optional embodiments, the organic carrier used in the seed layer slurry comprises the following components by weight percentage: ethyl cellulose: 10.0-16.0 wt%, methyl methacrylate and / or butyl methacrylate diacrylate resin: 6.0-9.0 wt%, thixotropic agent: 2.0-6.0 wt%, dispersant: 3.0-5.0 wt%, diethylene glycol butyl ether acetate: 43.0-50.0 wt%, dodecyl alcohol ester: 11.0-13.0 wt%, terpineol: 10.0-12.0 wt%, polydimethylsiloxane: 2.0 wt%; the organic carrier used in the base metal layer slurry comprises the following components by weight percentage: ethyl cellulose: 8.0-12.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin: 5.0 wt%, thixotropic agent: 1.0-1.5 wt%, dispersant: 6.0 wt%, diethylene glycol butyl ether acetate: 49.0-52.0 wt%. wt%, 12.5-13.0 wt% of alcohol ester dodecyl, 12.0-13.0 wt% of terpineol, and 2.0 wt% of polydimethylsiloxane. This application has at least the following technical effects:
[0015] 1) A first aspect of this application provides an electrode gate line, comprising a seed layer printed on the surface of a silicon wafer and a base metal layer superimposed on the seed layer. The electrode gate line of a predetermined height is formed by stacking the seed layer and the base metal layer. The base metal accounts for more than 68% of the conductive phase of the base metal layer, effectively reducing the silver consumption of the electrode gate line. In addition, at least one of the seed layer fine gate and the base metal layer fine gate is provided with a plurality of contact feet. The contact feet are distributed at intervals along the length direction of their corresponding fine gates, and the width of the contact feet in the linewidth direction of their respective fine gates is greater than the linewidth of their respective fine gates. The portion of the contact feet that exceeds the linewidth of their respective fine gates can be used to compensate for printing accuracy deviations. That is, when the printing deviation of the seed layer fine gate and the base metal layer fine gate is within the width range of the portion of the contact feet that exceeds the linewidth of their respective fine gates, the base metal layer fine gates can still overlap one-to-one with the seed layer fine gates, reducing the accuracy requirements of the printing operation and improving electrical conductivity.
[0016] 2) A second aspect of this application provides a method for preparing electrode grid lines, comprising preparing a seed layer screen and a base metal layer screen, and sequentially preparing a seed layer for a back electrode, a base metal layer for a back electrode, a seed layer for a front electrode, and a base metal layer for a front electrode, thereby obtaining back electrode grid lines and front electrode grid lines. At least one of the seed layer screen and the base metal layer screen has a contact foot pattern on its fine grid pattern to compensate for fine grid misalignment error and achieve good contact performance of the electrode grid lines in the stacked grid structure.
[0017] 3) A third aspect of this application provides a conductive paste, wherein corresponding seed layer paste and base metal layer paste are respectively provided for the seed layer and the base metal layer. The seed layer paste uses pure silver powder as the conductive phase. Silver has good bonding force with silicon wafer and can form a structurally stable Ag-Si alloy layer to achieve efficient tunneling of charge carriers. The base metal content in the conductive phase of the base metal layer paste exceeds 68%. Relying on the welding-tunneling function of the seed layer, the conductivity of the base metal is fully utilized to form an efficient longitudinal current conduction channel to achieve efficient current output. At the same time, it can also effectively reduce the overall silver consumption of the electrode grid lines. In specific implementation, the silver consumption of a single cell can be reduced by up to about 87%. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the description of the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 A partial structural schematic diagram of the seed layer screen pattern in an optional embodiment of the electrode grid line fabrication method provided in this application;
[0020] Figure 2 A partial structural schematic diagram of the base metal layer screen pattern in an optional embodiment of the electrode grid line fabrication method provided in this application.
[0021] Reference numerals: Main grid pattern 10, seed layer fine grid pattern 12, base metal layer fine grid pattern 21, contact foot pattern 30. Detailed Implementation
[0022] The embodiments of this implementation are described in detail below. These embodiments are only used to explain this implementation and should not be construed as limiting this implementation.
[0023] In the description of the embodiments of this application, it should be noted that all ranges disclosed in this application are to be understood to encompass any and all subranges included therein. For example, the stated range "30-100μm" should be considered to include any and all subranges that begin with a minimum value of 30μm or greater and end with a maximum value of 100μm or less, such as 35-58μm, or 60-97μm, or 77-100μm. Furthermore, all ranges disclosed in this application are also considered to include the endpoints of the ranges, unless otherwise expressly stated. For example, the ranges "20-80wt%", "20wt% to 80wt%", or "between 20wt% and 80wt%" should generally be considered to include the endpoints 20wt% and 80wt%.
[0024] Unless otherwise specified, in this article, ratio refers to mass ratio and percentage refers to mass percentage.
[0025] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0026] This application addresses the limited effectiveness of existing technologies in reducing silver consumption of electrode grids by simply increasing the number of fine grids and decreasing their linewidth. While using base metal powder to replace some or all of the silver powder in base metal pastes for printing the main and fine grids can significantly reduce silver consumption, base metal powders have poor oxidation resistance and electrical properties, as well as poor compatibility with silicon substrates. Furthermore, the high printing precision (±5μm) required for the overlap of the main and fine grids results in poor electrical properties of the obtained electrode grid lines, leading to unsatisfactory product yield. Therefore, this application explores a solution to minimize silver consumption of electrode grid lines as much as possible without compromising electrical performance and improving product yield. Specifically, by using a stacked gate process with a seed layer superimposed on a base metal layer, the traditional electrode grid structure is vertically segmented. The bottom seed layer uses traditional silver paste to reduce the barrier height, ensuring its bonding and contact performance with the silicon substrate, and achieving efficient carrier tunneling. The upper base metal layer forms good electrical contact with the seed layer, reducing the amount of silver powder used, and does not affect the continuous and efficient conduction of current.
[0027] Specifically, in order to achieve the above objectives, the technical solution adopted in this application is as follows:
[0028] A first aspect of this application provides an electrode gate line, comprising a seed layer printed on the surface of a silicon wafer and a base metal layer superimposed on the seed layer, wherein the base metal accounts for more than 68% of the conductive phase of the base metal layer, the seed layer includes a main gate and a seed layer fine gate, and the base metal layer includes base metal layer fine gates that are electrically connected to the seed layer fine gates one by one. At least one of the seed layer fine gates and the base metal layer fine gates is further provided with a plurality of contact feet, the contact feet being spaced apart along the length direction of their corresponding fine gates, and the width of the contact feet in the linewidth direction of their respective fine gates being greater than the linewidth of their respective fine gates.
[0029] Electrode grid lines of a predetermined height are formed by stacking a seed layer and a base metal layer. The base metal content in the conductive phase of the base metal layer exceeds 68%, effectively reducing the silver consumption of the electrode grid lines. In addition, at least one of the seed layer fine grid and the base metal layer fine grid is provided with several contact feet. The contact feet are distributed at intervals along the length direction of their corresponding fine grids, and the width of each contact foot in the linewidth direction of its respective fine grid is greater than the linewidth of its fine grid. The portion of the contact foot that exceeds the linewidth of its fine grid can be used to compensate for printing accuracy deviations. That is, when the printing deviation of the seed layer fine grid and the base metal layer fine grid is within the width range of the portion of the contact foot that exceeds the linewidth of its fine grid, the base metal layer fine grid can still overlap with the seed layer fine grid one by one, reducing the accuracy requirements of the printing operation and improving contact performance.
[0030] In practical implementation, the number of contact feet distributed on a single fine gate can be set to 20-100, and can be uniformly or non-uniformly distributed. The function of the contact feet is to compensate for the misalignment error when there is a misalignment between the seed layer fine gate and the base metal layer fine gate, forming additional contact points to achieve electrical contact between the seed layer and the base metal layer, thus forming an efficient longitudinal current conduction channel.
[0031] It is understandable that when both the seed layer and the base metal layer are provided with contact feet, the contact feet can be arranged in a one-to-one correspondence or can be arranged in a staggered manner.
[0032] Furthermore, the contact feet are evenly distributed between every two adjacent main gates, and the shape of the contact feet is one or more of the following: rhombus, square, ellipse, and linear.
[0033] Furthermore, the width of the contact foot in the linewidth direction of its respective fine grid is 30-100 μm, and the length of the contact foot in the length direction of its respective fine grid is 3-30 μm.
[0034] Specifically, the shape, size, and number of contact feet can be adjusted according to the length and linewidth of the fine grid lines and the wet weight of the seed layer fine grid and / or base metal layer fine grid. It is understood that when the wet weight is determined, the quality of the contact feet is also relatively determined. In this case, with a fixed thickness, the more contact feet there are, the smaller the size of a single contact angle will be. When the number of contact feet is small, the size of a single contact angle can be appropriately increased.
[0035] See Figures 1-2 The second aspect of this application provides a method for fabricating an electrode grid line as described in any of the preceding claims, comprising the following steps:
[0036] S1: A seed layer screen and a base metal layer screen are prepared according to the number and linewidth information of the main grid and fine grid of the electrode grid lines. The seed layer screen is a screen that combines the main grid pattern 10 and the seed layer fine grid pattern 12. The base metal layer screen only contains fine grid patterns 21. At least one of the seed layer screen and the base metal layer screen has a plurality of contact pin patterns 30 on the fine grid pattern 21. The contact pin patterns 30 are spaced apart along the length direction of the fine grid pattern 21, and the width of the contact pin pattern 30 is greater than the width of the fine grid pattern 21 in which it is located.
[0037] S2: Using the seed layer screen and conductive paste, the seed layer of the back electrode is screen printed on the back side of the silicon wafer. The printing pressure is 50 N / cm², the printing speed is 500 mm / s, and the wafer is dried and heat-treated.
[0038] S3: The base metal layer is superimposed on the seed layer in step S2 by screen printing using the base metal layer screen and conductive paste. The printing pressure is 50 N / cm² and the printing speed is 500 mm / s. After drying and heat treatment, the electrode grid lines of the back electrode are obtained.
[0039] S4: Referring to steps S2 and S3, the seed layer and the base metal layer are screen printed on the front side of the silicon wafer to obtain the electrode gate lines of the front electrode.
[0040] S5: A laser device is used to scan and enhance the conductivity of the electrode grid lines.
[0041] Specifically, the laser equipment is an infrared semiconductor laser, model number: DRM4XS-LIF-2000, with a spot diameter of 4.5Hm (hexagonal), operating parameters: power 17%, bias voltage 45V, air atmosphere, area scanning mode (perpendicular to the fine grating lines), scanning speed 55000mm / s, and frequency 100kHz.
[0042] A third aspect of this application provides a conductive paste for printing electrode grid lines as described in any of the preceding claims or for printing electrode grid lines prepared by the aforementioned method. The conductive paste comprises a seed layer paste for preparing the seed layer and a base metal layer paste for preparing the base metal layer. The conductive phase of the seed layer paste is silver powder, with a silver powder mass percentage of 20-80 wt%. The conductive phase of the base metal layer paste is base metal powder or a mixture of base metal powder and silver powder, with a base metal powder mass percentage of 60-90 wt% and a silver powder mass percentage of 0-30 wt%. The fineness of the seed layer paste is below 5 μm and its viscosity is 30-80 Pa·s. The fineness of the base metal layer paste is below 10 μm and its viscosity is 50-100 Pa·s.
[0043] Seed layer slurry with a fineness of less than 5μm can increase the slurry bulk density, enhance printing uniformity, improve wet weight stability, and at a viscosity of 30-80 Pa·s, the slurry has good leveling properties, which is beneficial to improving printing efficiency.
[0044] Furthermore, the silver powder is spherical, flake-shaped, or irregularly shaped, with a D50 particle size ranging from 1.2 to 1.8 μm and a tap density of 5.0 to 7.0 g / cm³. 3 Specific surface area 0.5-0.7 m² 2 / g, wherein the base metal powder is one or more selected from nickel powder, copper powder, tungsten powder, chromium powder, molybdenum powder, nickel-based alloy powder, copper-based alloy powder, silver-coated nickel powder, and silver-coated copper powder, with a D50 particle size range of 0.3-10μm and a tap density of 5.0-7.0g / cm³. 3 Specific surface area 0.5-2.5m² 2 / g.
[0045] Furthermore, the seed layer slurry also includes the following components by mass percentage: 0.5-6 wt% glass powder, 15-75 wt% organic carrier; the glass powder used in the seed layer slurry includes at least four of PbO, TeO2, Bi2O3, SiO2, Al2O3, ZnO and WO3.
[0046] Specifically, silver powder, glass powder, and organic carrier are pre-dispersed in a centrifugal degassing machine, and then ground in a three-roll mill to obtain the seed layer slurry with the above-mentioned fineness and viscosity.
[0047] Furthermore, the glass powder used in the seed layer slurry comprises the following components by mass percentage: 40wt% PbO, 2.0wt% SiO2, 30wt% TeO2, 20wt% Bi2O3, 3.0wt% ZnO and 5.0wt% WO3.
[0048] Specifically, TeO2 and Bi2O3 synergistically form a glass network, with high PbO content serving as a network modifier to suppress crystallization tendency, improve high-temperature fluidity, and ensure wetting and coating of the electrode / substrate during sintering. 5wt% WO3 refines grain boundaries, lowers densification temperature, and optimizes glass network connectivity by forming WO4²⁻ tetrahedra. The resulting electrode grid conductive network has good continuity and excellent contact performance.
[0049] In some embodiments, the base metal layer slurry further includes the following components by weight percentage: 0-3 wt% glass powder, 5-15 wt% organic carrier, wherein the base metal powder is one or more of nickel powder, copper powder, tungsten powder, chromium powder, molybdenum powder, nickel-based alloy powder, copper-based alloy powder, silver-coated nickel powder, and silver-coated copper powder.
[0050] Furthermore, the glass powder used in the base metal layer slurry includes at least five of the following: PbO, TeO2, Bi2O3, SiO2, Al2O3, ZnO, Cu2O, MnO, TiO2, and B2O3.
[0051] Specifically, the base metal powder or a mixture of base metal powder and pure silver powder, glass powder, and organic carrier are pre-dispersed in a centrifugal degassing machine, and then ground in a three-roll mill to obtain the base metal layer slurry with the above-mentioned fineness and viscosity.
[0052] Furthermore, the glass powder used in the base metal layer slurry comprises the following components by mass percentage: 10wt% PbO, 40wt% SiO2, 2.0wt% TeO2, 5.0wt% Bi2O3, 3.0wt% ZnO, 4.0wt% Al2O3, 20wt% Cu2O, 5.0wt% TiO2, 10wt% MnO, and 1.0wt% B2O3.
[0053] [SiO4] was constructed using SiO2 as the main network form. 4- The tetrahedral framework, with B2O3 assisting in the formation of [BO3] / [BO4] groups, constructs the basic glass phase structure. Cu2O, PbO, and Bi2O3 serve as strong network modifiers, enhancing flow and lowering the glass transition temperature. Al2O3, TiO2, and ZnO act as functional ions, synergistically improving chemical durability and thermal stability. At the same time, the high Cu2O content can also enhance the conductivity of the slurry system, compensating for the decline in conductivity caused by the oxidation of base metals.
[0054] Understandably, the reason why the glass powder used in the seed layer slurry differs from that used in the base metal layer slurry lies in the different conductive phases in the two slurries. In the seed layer slurry, the conductive phase is pure silver powder. Based on the physicochemical properties of silver powder, the selection of glass powder primarily considers its affinity with silver powder, improving the bonding between the glass powder system and the silver powder, and enhancing the contact performance of the electrode grid lines. In contrast, the conductive phase in the base metal layer slurry also includes base metal powder. The selection of glass powder must also consider the poor conductivity and easy oxidation of base metal powder. Therefore, it is necessary to select components that can help improve the system's oxidation resistance, thermal stability, conductivity, and reduce sintering temperature, such as the addition of functional oxides like Al2O3, TiO2, ZnO, and Cu2O.
[0055] Further, the organic carrier used in the seed layer slurry comprises the following components by weight percentage: ethyl cellulose: 10.0-16.0 wt%, methyl methacrylate and / or butyl methacrylate diacrylate resin: 6.0-9.0 wt%, thixotropic agent: 2.0-6.0 wt%, dispersant: 3.0-5.0 wt%, diethylene glycol butyl ether acetate: 43.0-50.0 wt%, dodecyl alcohol ester: 11.0-13.0 wt%, terpineol: 10.0-12.0 wt%, polydimethylsiloxane: 2.0 wt%;
[0056] The organic carrier used in the base metal layer slurry comprises the following components by weight percentage: ethyl cellulose: 8.0-12.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin: 5.0 wt%, thixotropic agent: 1.0-1.5 wt%, dispersant: 6.0 wt%, diethylene glycol butyl ether acetate: 49.0-52.0 wt%, dodecyl alcohol ester: 12.5-13.0 wt%, terpineol: 12.0-13.0 wt%, and polydimethylsiloxane: 2.0 wt%.
[0057] The following examples will further illustrate this application.
[0058] Unless otherwise specified, all reagents and materials used in the following examples and comparative examples are commercially available. All reagents and raw materials used in the examples and comparative examples of this application are commercially available.
[0059] Example 1
[0060] Example 1 provides a seed layer slurry:
[0061] Raw material ratio: By mass percentage, silver powder 80wt%, glass powder 3wt%, and organic carrier 17wt%. The silver powder is spherical with a D50 particle size of 1.4μm, a tap density of 6.0g / cm³, and a specific surface area of 0.70 m² / g. The glass powder is formulated according to the following mass ratio: PbO: 40wt%, SiO2: 2.0wt%, TeO2: 30wt%, Bi2O3: 20wt%, ZnO: 3.0wt%, and WO3: 5.0wt%.
[0062] The organic carrier is composed of the following components by mass ratio: ethyl cellulose (DOW™ N4): 10.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin (PARALOID™ B-66): 6.0 wt%, thixotropic agent (Kushu Chemical ET-2020): 2 wt%, dispersant (AkzoDuomeen TDO): 5.0 wt%, diethylene glycol butyl ether acetate: 50.0 wt%, dodecyl alcohol ester: 13.0 wt%, terpineol: 12.0 wt%, and polydimethylsiloxane (Dow Corning, viscosity grade 20): 2.0 wt%.
[0063] Preparation process: The raw materials were added to a centrifugal degassing machine in sequence and pre-dispersed at a speed of 1800 rpm for 2 minutes; then transferred to a three-roll mill, with the distance between the feed roller and the middle roller set to 20 μm and the distance between the middle roller and the discharge roller set to 5 μm. The feed roller speed was controlled at 200 rpm, the middle roller speed at 2600 rpm and the discharge roller speed at 300 rpm, and the milling was repeated 6 times.
[0064] Performance testing: The fineness of the prepared seed layer slurry was 3 μm and the viscosity was 55 Pa·s.
[0065] Application: The seed layer slurry is screen-printed onto a battery silicon wafer, with a printing pressure of 50 N / cm² and a printing speed of 500 mm / s.
[0066] Example 2
[0067] Example 2 provides a seed layer slurry. The only difference between Example 2 and Example 1 is the raw material ratio: by mass percentage, silver powder 60wt%, glass powder 3wt%, and organic carrier 37wt%.
[0068] The organic carrier is composed of the following components by mass ratio: ethyl cellulose (DOW™ N4): 13.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin (PARALOID™ B-66): 7.0 wt%, thixotropic agent (Kushu Chemical ET-2020): 4 wt%, dispersant (AkzoDuomeen TDO): 4.0 wt%, diethylene glycol butyl ether acetate: 47.0 wt%, dodecyl alcohol ester: 12.0 wt%, terpineol: 11.0 wt%, and polydimethylsiloxane (Dow Corning, viscosity grade 20): 2.0 wt%.
[0069] All other conditions, preparation process, performance and application are the same as in Example 1, with a viscosity of 50 Pa·s.
[0070] Example 3
[0071] Example 3 provides a seed layer slurry. The difference between Example 3 and Example 1 lies in the raw material ratio: by mass percentage, 40 wt% silver powder, 5 wt% glass powder, and 55 wt% organic carrier. The silver powder is irregularly spherical with a D50 particle size of 1.6 μm, a tap density of 5.7 g / cm³, and a specific surface area of 0.60 m² / g. The preparation process is the same as in Example 1. The resulting seed layer slurry has a fineness of 3 μm and a viscosity of 48 Pa·s. All other conditions are the same as in Example 1.
[0072] The organic carrier is composed of the following components by mass ratio: ethyl cellulose (DOW™ N4): 16.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin (PARALOID™ B-66): 9.0 wt%, thixotropic agent (Kushu Chemical ET-2020): 6 wt%, dispersant (AkzoDuomeen TDO): 3.0 wt%, diethylene glycol butyl ether acetate: 43.0 wt%, dodecyl alcohol ester: 11.0 wt%, terpineol: 10.0 wt%, and polydimethylsiloxane (Dow Corning, viscosity grade 20): 2.0 wt%.
[0073] Example 4
[0074] Example 4 provides a base metal layer slurry:
[0075] Raw material ratio: By mass percentage, 75wt% base metal powder (nickel powder and copper powder mixed in a mass ratio of 3:2), 15wt% silver powder, 2wt% glass powder, and 8wt% organic carrier. The base metal powder has a D50 particle size of 3μm, a tap density of 6.5g / cm³, and a specific surface area of 1.2m² / g; the silver powder specifications are the same as those in Example 1; the glass powder is prepared according to the following ratio: PbO: 10wt%, SiO2: 40wt%, TeO2: 2.0wt%, Bi2O3: 5.0wt%, ZnO: 3.0wt%, Al2O3: 4.0wt%, Cu2O: 20wt%, TiO2: 5.0wt%, MnO: 10wt%, and Bi2O3: 1.0wt%.
[0076] The organic carrier is composed of the following components by mass ratio: ethyl cellulose (DOW™ N4): 8.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin (PARALOID™ B-66): 5.0 wt%, thixotropic agent (Kushu Chemical ET-2020): 1.0 wt%, dispersant (AkzoDuomeen TDO): 6.0 wt%, diethylene glycol butyl ether acetate: 52.0 wt%, dodecyl alcohol ester: 13.0 wt%, terpineol: 13.0 wt%, and polydimethylsiloxane (Dow Corning, viscosity grade 20): 2.0 wt%.
[0077] Preparation process: The raw materials were added to a centrifugal degassing machine in sequence and pre-dispersed for 2 minutes at a speed of 1800 rpm; then transferred to a three-roll mill, with the distance between the feed roller and the middle roller set to 20 μm and the distance between the middle roller and the discharge roller set to 5 μm. The mill was circulated and ground 6 times at a normal speed.
[0078] Performance testing: The fineness of the prepared base metal layer slurry was 6 μm and the viscosity was 75 Pa·s.
[0079] Application: After the seed layer slurry is printed, it is superimposed on the seed layer slurry and sent to sintering. The heating rate is set to 5℃ / min and the maximum temperature is 800℃.
[0080] Example 5
[0081] Example 5 provides a base metal layer slurry:
[0082] Raw material ratio: 85wt% base metal powder (silver-coated nickel powder: 10wt% silver + 90wt% nickel), 5wt% silver powder, 1wt% glass powder, and 9wt% organic carrier. The base metal powder has a D50 particle size of 3μm, a tap density of 6.8g / cm³, and a specific surface area of 1.8m² / g; the silver powder specifications are the same as those in Example 4; the glass powder formulation is the same as in Example 4.
[0083] The organic carrier has the following composition by mass: ethyl cellulose (DOW™ N4): 12.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin (PARALOID™ B-66): 5.0 wt%, thixotropic agent (Kushu Chemical ET-2020): 1.5 wt%, dispersant (AkzoDuomeen TDO): 6.0 wt%, diethylene glycol butyl ether acetate: 49.0 wt%, dodecyl alcohol ester: 12.5 wt%, terpineol: 12.0 wt%, and polydimethylsiloxane (Dow Corning, viscosity grade 20): 2.0 wt%.
[0084] Preparation process: centrifuge degassing machine speed 1800 rpm, pre-dispersion for 2 minutes; three-roll mill grinding, cyclic grinding 6 times.
[0085] Performance testing: The fineness of the prepared base metal layer slurry was 7 μm and the viscosity was 82 Pa·s.
[0086] Application: After the seed layer slurry is printed, it is superimposed on the seed layer slurry and sent to sintering. The heating rate is set to 5℃ / min and the maximum temperature is 800℃.
[0087] Example 6
[0088] Example 6 provides a base metal layer slurry:
[0089] Raw material ratio: 90wt% base metal powder (nickel-based alloy powder), 1wt% glass powder, and 9wt% organic carrier. The base metal powder has a D50 particle size of 3μm, a tap density of 6.8g / cm³, and a specific surface area of 1.8m² / g; the glass powder and organic carrier formulations are the same as in Example 4.
[0090] Preparation process: Same as in Example 4.
[0091] Performance testing: The fineness of the prepared base metal layer slurry was 7 μm and the viscosity was 82 Pa·s.
[0092] Application: After the seed layer slurry is printed, it is superimposed on the seed layer slurry and sent to sintering. The heating rate is set to 5℃ / min and the maximum temperature is 800℃.
[0093] The embodiments 1-3 and 4-6 are combined and applied according to the following table:
[0094] Seed layer slurry Base metal layer slurry Seed layer slurry Base metal layer slurry 1# Example 1 Example 4 6# Example 2 Example 6 2# Example 1 Example 5 7# Example 3 Example 4 3# Example 1 Example 6 8# Example 3 Example 5 4# Example 2 Example 4 9# Example 3 Example 6 5# Example 2 Example 5
[0095] The preparation process of the above-mentioned solar cells #1-#9 includes the following steps: S1: Based on the silicon wafer dimensions of 182mm width and 210mm length, the corresponding fine grid printing length is 180mm, line width is 25-30mm, spacing is 0.9-1.0mm, and the quantity is 228. The main grid printing length is 209mm, line width is 50-60mm, spacing is 10-11mm, and the quantity is 16. Prepare the seed layer screen (see...). Figure 1 ) and base metal layer mesh (see Figure 1 The contact foot pattern 30 is disposed on the seed layer fine gate pattern 12 and the base metal layer fine gate pattern 21, and is evenly distributed between the spacing of two adjacent main gate patterns 10. Each spacing is provided with 2-5 contact feet, which are rhomboid in shape and have a width of 65μm and a length of 18μm in the line width direction.
[0096] S2: Following the printing order of the back seed layer, the back base metal layer, the front seed layer, and the front base metal layer, the electrode grid lines of the back electrode and the front electrode are obtained.
[0097] S3: Drying, sintering below 800℃, laser-assisted enhancement, using an infrared semiconductor laser with a spot diameter of 4.5Hm (hexagonal). Specific parameters are set as follows: power 17%, bias voltage 45V, air atmosphere, surface scanning mode (perpendicular to the fine grating line), scanning speed 55000mm / s, frequency 100kHz.
[0098] Comparative Example
[0099] The process employs a multi-stage printing process for the main gate and fine gate. First, a main gate paste with a conventional silver content of 85wt% is used to print the back main gate on the back of the silicon wafer. Then, a fine gate paste with a silver content of 89wt% is used to print the back fine gate. The above steps are then repeated on the front side of the silicon wafer to prepare the front main gate and the front fine gate.
[0100] The comparison results of silver consumption between Examples 1-6 and the comparative conductive paste are as follows:
[0101]
[0102] The comparative printing method is the same as that for solar cells #1-#9 mentioned above.
[0103] The conversion efficiency, open-circuit voltage, short-circuit current, fill factor, and series resistance of the solar cells (#1-#9) obtained in the above steps and the cells prepared in the comparative example were tested using a commercially available IV and EL tester. The data from the comparative example were used as the standard values, as shown in the table below:
[0104] project Eff / % Uoc / V Isc / A FF / % Rs / Ω Comparative Example 27.2 0.7372 16.376 86.20 0.588
[0105] The differences in various data points between photovoltaic cells #1-#9 and the comparative example are shown in the table below:
[0106] project ΔEff / % ΔUoc / V ΔIsc / A ΔFF / % ΔRs / Ω 1# +0.046 +0.0004 +0.0024 +0.100 -0.00003 2# +0.037 0.0000 +0.0011 +0.060 0.00000 3# +0.023 +0.0001 +0.0020 0.000 -0.00001 4# +0.033 0.0000 +0.0030 +0.080 -0.00005 5# +0.024 +0.0001 +0.0025 +0.000 -0.00002 6# +0.002 0.0000 +0.0030 -0.020 -0.00002 7# +0.028 +0.0002 +0.0038 0.000 -0.00001 8# +0.016 0.0000 +0.0022 -0.022 -0.00002 9# +0.003 -0.0002 +0.0010 -0.040 +0.00002
[0107] The total silver consumption of the electrode grid lines for the aforementioned 1#-9# solar cells and the comparative solar cells is calculated to be:
[0108] Total silver consumed (mg) Comparative Example 68.9 1# 37.65 2# 30.15 3# 26.40 4# 28.05 5# 20.55 6# 16.80 7# 20.05 8# 12.55 9# 8.80
[0109] The test data above shows that using Examples 3 and 6 as seed layer slurry and base metal layer slurry, respectively, resulted in the lowest silver consumption of the electrode assembly. Even with a total silver consumption of only 13% of the comparative example, the photoelectric efficiency of the resulting #9 photovoltaic cell was still 0.003% higher than the comparative example. Furthermore, using Examples 1 and 4 as seed layer slurry and base metal layer slurry, respectively, increased the silver consumption of the resulting electrode grid to 37.65 mg. At this point, the total silver consumption of the resulting electrode grid was only 55% of the comparative example. The electrical performance indicators of the resulting #1 photovoltaic cell were significantly improved compared to the comparative example. This significantly reduced the silver consumption of the electrode assembly while also significantly improving the electrical performance of the corresponding solar cell, providing a powerful solution for cost reduction and efficiency improvement in the photovoltaic industry, and possessing considerable industrial application prospects and economic benefits.
[0110] Although embodiments of this implementation have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this implementation, the scope of which is defined by the claims and their equivalents.
Claims
1. An electrode grid line, characterized in that, The device includes a seed layer printed on the surface of a silicon wafer and a base metal layer superimposed on the seed layer. The base metal content in the conductive phase of the base metal layer is greater than 68%. The seed layer includes a main gate and a seed layer fine gate. The base metal layer includes base metal layer fine gates that are electrically connected to the seed layer fine gates one by one. At least one of the seed layer fine gates and the base metal layer fine gates is further provided with a plurality of contact feet. The contact feet are spaced apart along the length direction of their corresponding fine gates, and the width of the contact feet in the linewidth direction of their respective fine gates is greater than the linewidth of their respective fine gates.
2. The electrode grid line according to claim 1, characterized in that, The contact feet are evenly distributed between every two adjacent main grids, and the shape of the contact feet is one or more of the following: rhombus, square, ellipse, and linear.
3. The electrode grid line according to claim 1, characterized in that, The width of the contact foot in the linewidth direction of its respective fine grid is 30-100μm, and the length of the contact foot in the length direction of its respective fine grid is 3-30μm.
4. A method for preparing electrode grid lines as described in any one of claims 1-3, characterized in that, Includes the following steps: S1: Prepare a seed layer screen and a base metal layer screen according to the number and linewidth information of the main grid and fine grid of the electrode grid lines. The seed layer screen is a screen that combines the main grid pattern and the fine grid pattern. The base metal layer screen only contains the fine grid pattern. At least one of the seed layer screen and the base metal layer screen has a plurality of contact pin patterns on the fine grid pattern. The contact pin patterns are distributed at intervals along the length direction of the fine grid pattern, and the width of the contact pin pattern is greater than the width of the fine grid pattern in which it is located. S2: Using the seed layer screen and conductive paste, screen print the seed layer of the back electrode on the back side of the silicon wafer. The printing pressure is 50 N / cm², and the printing speed is 500 mm / s. After drying, perform heat treatment. S3: Using the base metal layer screen and conductive paste, screen print the base metal layer onto the seed layer in step S2. The printing pressure is 50 N / cm², and the printing speed is 500 mm / s. After drying, perform heat treatment to obtain the electrode grid lines of the back electrode. S4: Referring to steps S2 and S3, screen print the seed layer and the base metal layer on the front side of the silicon wafer to obtain the electrode grid lines of the front electrode.
5. A conductive paste for printing electrode grid lines as described in any one of claims 1-3 or electrode grid lines prepared by the method for preparing electrode grid lines according to claim 4, characterized in that, The conductive paste includes a seed layer paste for preparing the seed layer and a base metal layer paste for preparing the base metal layer. The conductive phase of the seed layer paste is silver powder, and the silver powder has a mass percentage content of 20-80 wt% in the seed layer paste. The conductive phase of the base metal layer paste is base metal powder or a mixture of base metal powder and silver powder, and the base metal powder has a mass percentage content of 60-90 wt% in the base metal layer paste. The silver powder has a mass percentage content of 0-30 wt% in the base metal layer paste. The fineness of the seed layer paste is below 5 μm, and its viscosity is 30-80 Pa·s. The fineness of the base metal layer paste is below 10 μm, and its viscosity is 50-100 Pa·s.
6. The conductive paste according to claim 5, characterized in that, The silver powder is spherical, flake-shaped, or irregularly shaped, with a D50 particle size ranging from 1.2 to 1.8 μm and a tap density of 5.0 to 7.0 g / cm³. 3 Its specific surface area is 0.5-0.7 m². 2 / g, wherein the base metal powder is one or more selected from nickel powder, copper powder, tungsten powder, chromium powder, molybdenum powder, nickel-based alloy powder, copper-based alloy powder, silver-coated nickel powder, and silver-coated copper powder, with a D50 particle size range of 0.3-10μm and a tap density of 5.0-7.0g / cm³. 3 Its specific surface area is 0.5-2.5 m². 2 / g.
7. The conductive paste according to claim 5, characterized in that, The seed layer slurry further includes the following components by mass percentage: 0.5-6 wt% glass powder and 15-75 wt% organic carrier; the glass powder used in the seed layer slurry includes at least four of the following: PbO, TeO2, Bi2O3, SiO2, Al2O3, ZnO, and WO3.
8. The conductive paste according to claim 7, characterized in that, The glass powder used in the seed layer slurry comprises the following components by mass percentage: 40wt% PbO, 2.0wt% SiO2, 30wt% TeO2, 20wt% Bi2O3, 3.0wt% ZnO and 5.0wt% WO3.
9. The conductive paste according to claim 7, characterized in that, The base metal layer slurry further includes the following components by mass percentage: 0-3 wt% glass powder, 5-15 wt% organic carrier, wherein the glass powder used in the base metal layer slurry includes at least five of the following: PbO, TeO2, Bi2O3, SiO2, Al2O3, ZnO, Cu2O, MnO, TiO2 and B2O3.
10. The conductive paste according to claim 9, characterized in that, The glass powder used in the base metal layer slurry comprises the following components by mass percentage: 10wt% PbO, 40wt% SiO2, 2.0wt% TeO2, 5.0wt% Bi2O3, 3.0wt% ZnO, 4.0wt% Al2O3, 20wt% Cu2O, 5.0wt% TiO2, 10wt% MnO, and 1.0wt% B2O3.
11. The conductive paste according to claim 9, characterized in that, The organic carrier used in the seed layer slurry comprises the following components by weight percentage: ethyl cellulose: 10.0-16.0 wt%, methyl methacrylate and / or butyl methacrylate, and diacrylate resin. 6.0-9.0 wt%, thixotropic agent: 2.0-6.0 wt%, dispersant: 3.0-5.0 wt%, diethylene glycol butyl ether acetate: 43.0-50.0 wt%, dodecyl alcohol ester: 11.0-13.0 wt%, terpineol: 10.0-12.0 wt%, polydimethylsiloxane: 2.0 wt%; the organic carrier used in the base metal layer slurry comprises the following components by weight percentage: ethyl cellulose: 8.0-12.0 wt%, methyl methacrylate / butyl methacrylate diacrylate resin: 5.0 wt%, thixotropic agent: 1.0-1.5 wt%, dispersant: 6.0 wt%, diethylene glycol butyl ether acetate: 49.0-52.0 wt%, dodecyl alcohol ester: 12.5-13.0 wt%, terpineol: 12.0-13.0 wt%, polydimethylsiloxane: 2.0 wt%.
Citation Information
Cited By
Metallization slurry, conductive thin film, preparation method of conductive thin film and metallization structure