Lithium iron phosphate material as well as preparation method and application thereof
By constructing a nanoscale oxide protective layer in lithium iron phosphate materials using low-melting-point metal components and combining large and small particle gradation, the problem of balancing rate performance and high compaction density in lithium iron phosphate materials was solved, thus achieving the preparation of high-performance and high-stability lithium iron phosphate materials.
Patent Information
- Application Number
- CN202511690948.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-18
- Publication Date
- 2026-01-13
AI Technical Summary
Existing lithium iron phosphate materials cannot simultaneously achieve high rate performance and high compaction density, and existing modification methods can affect the cycling performance of the materials.
By utilizing the melting, wetting, and subsequent oxidation behavior of low-melting-point metal components under specific conditions, a dense and uniform nanoscale oxide protective layer is constructed. Through the gradation of large and small particles, combined with an integrated process of mixing-sintering-oxidation, the coating process and the synthesis of lithium iron phosphate are completed simultaneously.
It improves the electronic conductivity and structural stability of the material, achieves a balance between high solid density and excellent high-rate charge-discharge performance and cycle performance, simplifies the process, and is suitable for large-scale production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application belongs to the field of new energy technology, specifically relating to a lithium iron phosphate material, its preparation method, and its application. Background Technology
[0002] Lithium iron phosphate (LiFePO4) has become an important cathode material in the fields of power batteries and energy storage batteries due to its advantages such as high safety, long cycle life and low cost. However, its intrinsic electronic conductivity and ionic conductivity are relatively low, which limits its high-rate performance.
[0003] To address this issue, conventional techniques typically employ carbon coating or nano-sizing strategies. While carbon coating can improve electronic conductivity, it reduces the material's compaction density and volumetric energy density; while nano-sizing can shorten ion diffusion paths, it exacerbates side reactions, affects cycling performance, and complicates electrode fabrication.
[0004] There are some existing methods for coating with metals or metal oxides, but these methods often suffer from problems such as uneven coating, complex processes, or damage to the coating structure during high-temperature sintering, ultimately affecting cycle performance.
[0005] Therefore, it is of great significance to develop a simple process for preparing lithium iron phosphate materials that achieves uniform coating, high rate performance, high compaction density, and good cycle performance. Summary of the Invention
[0006] This application provides a lithium iron phosphate material, its preparation method, and its application, to solve the problems in the prior art where the rate performance and high compaction density of lithium iron phosphate materials cannot be simultaneously achieved, and existing modification methods can affect the material's cycle performance.
[0007] In a first aspect, this application provides a method for preparing lithium iron phosphate material, comprising the following steps: S1, mix lithium source, iron source, phosphorus source and carbon source to form a slurry, spray dry to obtain spray material, the spray material includes first particles with a particle size Dv50 of 3-6μm and second particles with a particle size Dv50 of 400-1000nm; S2, Under a protective atmosphere, the spray material is mixed with a low-melting-point metal component to obtain a mixture; wherein the melting point of the low-melting-point metal component is 150-700℃; S3, the mixture is sintered under a protective atmosphere and oxidized in an oxygen-containing atmosphere to obtain the lithium iron phosphate material.
[0008] In one optional embodiment, in S2, the amount of the low-melting-point metal component accounts for 0.1%-4% of the mass of the spray material; And / or, the low-melting-point metal component includes at least one of elemental aluminum, zinc, magnesium, bismuth, lead, tin, cadmium, indium, and alloys containing the above elements; Optionally, the low-melting-point metal component includes at least one of elemental bismuth, elemental tin, tin alloys, aluminum alloys, zinc alloys, and magnesium alloys.
[0009] In one alternative embodiment, in S3, the oxidation treatment is carried out at a temperature of 100-200°C for 2-4 hours.
[0010] In an optional embodiment, in S3, the sintering is segmented sintering, the segmented sintering comprising: First stage sintering: temperature 200-300℃, time 1-2h; Second stage sintering: temperature 350-450℃, time 2-3h; The third stage of sintering: the temperature is 700-850℃, and the time is 6-10h.
[0011] In one optional embodiment, the first and second particles in the spray material are separately subjected to subsequent steps S2 and S3 to obtain large lithium iron phosphate particles and small lithium iron phosphate particles, respectively. Optionally, the sintering temperature of the third stage corresponding to the first particle is 750-850℃; the sintering temperature of the third stage corresponding to the second particle is 700-750℃.
[0012] In one optional embodiment, the mass ratio of the large lithium iron phosphate particles to the small lithium iron phosphate particles is 1:9 to 9:1.
[0013] In an optional embodiment, in S1, the molar ratio of Li:Fe:P in the mixing and pulping step is 1-1.1:0.95-1.05:0.95-1.05; And / or, the amount of carbon source added is 5%-30% of the mass of iron; And / or, the mixing and pulping process further includes a grinding step, grinding the pulp until the particle size Dv50 is 200-400 nm; And / or, the spray drying is a two-fluid spray drying.
[0014] Secondly, this application provides a lithium iron phosphate material prepared by the above-described preparation method.
[0015] Thirdly, this application provides a secondary battery comprising the aforementioned lithium iron phosphate material.
[0016] Fourthly, this application provides an electrical device including the aforementioned secondary battery.
[0017] The technical solution of this application has the following advantages: This application provides a method for preparing lithium iron phosphate (LFP) materials. This method utilizes the melting, wetting, and subsequent oxidation behavior of low-melting-point metal components under specific conditions to construct a dense and uniform nanoscale oxide protective layer, effectively improving the material's electronic conductivity and structural stability. Through the gradation of large and small particles, the LFP material possesses both high compaction density and excellent high-rate charge-discharge and cycle performance. Furthermore, the integrated "mixing-sintering-oxidation" process simultaneously completes the coating process with the LFP synthesis process, eliminating the need for complex post-processing coating steps. This short process flow is suitable for large-scale production. Specifically, this application utilizes the melting characteristics of low-melting-point metal components at the LFP sintering temperature. The molten liquid metal, with its low surface tension, can effectively wet the surface of LFP particles, forming an extremely uniform 2-5 nm nanoscale metal coating through adsorption, spreading, and even vaporization and recondensation. This coating is then transformed into a structurally stable metal oxide coating layer through low-temperature oxidation. Compared to existing metal oxide coating methods, this method can form a denser and more uniform coating layer, and the steps are simpler. This layer can suppress side reactions of the electrolyte on the active material and inhibit cracking caused by repeated volume expansion and contraction of large particles during charge and discharge, thus improving cycle performance. By limiting the size of the first and second particles in the spray material, the compaction density can be improved. The first particle has a secondary spherical structure, and the lithium iron phosphate inside the first particle is a micron-sized spherical secondary particle or a solid primary particle formed by the agglomeration of primary nanoparticles. Its surface is coated with a dense nano-sized metal oxide layer, which has a high compaction density. The second particle has a smaller particle size, which has the following advantages: 1. Small particles can effectively fill the gaps between large particles, reduce electrode porosity, and improve compaction density. 2. The smaller particle size shortens the diffusion distance of lithium ions in the solid phase, accelerates the ion transport rate, and improves rate performance. 3. Small particles provide a larger specific surface area, increase the number of reactive sites at the electrode / electrolyte interface, improve interfacial reaction kinetics, and improve low-temperature performance. 4. The filling of small particles makes the electrode structure more dense and uniform, enhances the bonding force between particles, reduces particle shedding during charge and discharge cycles, and improves cycle life. It suppresses electrode expansion and maintains structural integrity. The combination of the first and second particles achieves a balance between compaction density, rate performance, and cycle performance, meeting the needs of different application scenarios.
[0018] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Detailed Implementation
[0019] The technical solutions in the embodiments of this application are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are intended to cover non-exclusive inclusion.
[0021] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.
[0022] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0023] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0024] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0025] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).
[0026] The following provides a detailed description of the lithium iron phosphate material, its preparation method, and its applications provided in this application.
[0027] As described in the background section, the rate performance and high compaction density of lithium iron phosphate materials cannot be simultaneously achieved, and existing modification methods can affect the material's cycle performance.
[0028] To address the problems existing in the aforementioned related technologies, according to one aspect of this application, a method for preparing lithium iron phosphate material is provided, comprising the following steps: S1, mix lithium source, iron source, phosphorus source and carbon source to form a slurry, spray dry to obtain spray material, the spray material includes first particles with a particle size Dv50 of 3-6μm and second particles with a particle size Dv50 of 400-1000nm; S2, Under a protective atmosphere, the spray material is mixed with a low-melting-point metal component to obtain a mixture; wherein the melting point of the low-melting-point metal component is 150-700℃; S3, the mixture is sintered under a protective atmosphere and oxidized in an oxygen-containing atmosphere to obtain the lithium iron phosphate material.
[0029] As an example, the particle size Dv50 of the first particle can be 3μm, 4μm, 5μm, 6μm, or within any range of the above values; the particle size Dv50 of the second particle can be 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, or within any range of the above values. The melting point of the low-melting-point metal component is 150℃, 200℃, 300℃, 400℃, 500℃, 600℃, 700℃, or within any range of the above values.
[0030] Based on the aforementioned technical means, this application utilizes the melting, wetting, and subsequent oxidation behavior of low-melting-point metal components under specific conditions to construct a dense and uniform nanoscale oxide protective layer, effectively improving the electronic conductivity and structural stability of the material. Through the gradation of large and small particles, the lithium iron phosphate material possesses both high compaction density and excellent high-rate charge-discharge performance and cycle performance. Furthermore, the integrated "mixing-sintering-oxidation" process simultaneously completes the coating process with the lithium iron phosphate synthesis process, eliminating the need for complex post-processing coating steps, resulting in a short process flow suitable for large-scale production. Specifically, this application utilizes the melting characteristics of low-melting-point metal components at the sintering temperature of lithium iron phosphate. The molten liquid metal, with its low surface tension, can effectively wet the surface of lithium iron phosphate particles, forming an extremely uniform 2-5nm nanoscale metal coating through adsorption, spreading, and even vaporization and recondensation. This coating is then transformed into a structurally stable metal oxide coating layer through low-temperature oxidation. Compared to existing metal oxide coating methods, this approach can form a denser and more uniform coating layer, and the steps are simpler. This layer can suppress side reactions of the electrolyte on the active material and inhibit cracking caused by repeated volume expansion and contraction of large particles during charge and discharge, thus improving cycle performance. By limiting the size of the first and second particles in the spray material, the compaction density can be improved. The first particle has a secondary spherical structure, and the lithium iron phosphate inside the first particle is a micron-sized spherical secondary particle or a solid primary particle formed by the agglomeration of primary nanoparticles. Its surface is coated with a dense nano-sized metal oxide layer, which has a high compaction density. The second particle has a smaller particle size, which has the following advantages: 1. Small particles can effectively fill the gaps between large particles, reduce electrode porosity, and improve compaction density. 2. The smaller particle size shortens the diffusion distance of lithium ions in the solid phase, accelerates the ion transport rate, and improves rate performance. 3. Small particles provide a larger specific surface area, increase the number of reactive sites at the electrode / electrolyte interface, improve interfacial reaction kinetics, and improve low-temperature performance. 4. The filling of small particles makes the electrode structure more dense and uniform, enhances the bonding force between particles, reduces particle shedding during charge and discharge cycles, and improves cycle life. It suppresses electrode expansion and maintains structural integrity. The combination of the first and second particles achieves a balance between compaction density, rate performance, and cycle performance, meeting the needs of different application scenarios.
[0031] In one optional embodiment, in S2, the amount of the low-melting-point metal component accounts for 0.1%-4% of the mass of the spray material; As an example, the amount of the low-melting-point metal component is 0.1%, 0.2%, 0.4%, 0.5%, 0.7%, 0.9%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% of the mass of the spray material, or within any of the above values.
[0032] Based on the aforementioned technical means, this application, by limiting the amount of low-melting-point metal components, can ensure the coating effect while avoiding any impact on the material's electrical properties. If the amount is too small, uncoated areas will exist, failing to achieve the desired coating effect; if the amount is too large, the coating layer will be too thick, affecting lithium-ion insertion / extraction and subsequent oxidation behavior, and the free metal oxides present between particles will also affect the material's performance.
[0033] In one alternative embodiment, the low-melting-point metal component includes at least one of elemental aluminum, zinc, magnesium, bismuth, lead, tin, cadmium, indium, and alloys comprising the above elements; In one alternative embodiment, the low-melting-point metal component preferably includes at least one of elemental bismuth, elemental tin, tin alloys, aluminum alloys, zinc alloys, and magnesium alloys.
[0034] It should be noted that the alloys involved in this application may include not only the low-melting-point elemental components listed above, but also other elemental components that form alloys with it, as long as the melting point of the alloy components can meet the above-mentioned limitations.
[0035] Based on the aforementioned technical methods, in the modification of lithium iron phosphate (LiFePO4, LFP) cathode materials, coating with multiple oxides, compared to coating with a single oxide, has the core advantage of simultaneously addressing the performance shortcomings of LFP materials in multiple dimensions, such as electronic conductivity, ion migration efficiency, cycle stability, and interface stability, through the "functional complementarity" of different oxides, achieving a synergistic enhancement effect of "1+1>2". While a single metal element corresponds to a single oxide coating layer, alloys can be used to achieve co-coating with multiple oxides.
[0036] For example, a single oxide coating may crack or peel off due to mechanical stress (volume changes during charge and discharge) or chemical corrosion (electrolyte decomposition products), leading to accelerated performance degradation in the later stages of cycling (e.g., capacity retention <80% after 500 cycles). Multi-oxide coatings can form composite coatings: corrosion-resistant, high-mechanical-strength oxides (such as Al₂O₃) resist electrolyte erosion, while flexible oxides (Bi₂O₃) buffer volume stress, preventing coating failure. Al₂O₃ (corrosion resistant) + Bi₂O₃ (buffering). Another example is antimony-tin alloys (5%-10% antimony by mass), which, after oxidation, form metal-doped electronic conductor oxides. Antimony doping introduces charge carriers (such as free electrons and holes), significantly improving the electronic conductivity of the coating compared to pure tin dioxide, thereby enhancing material performance.
[0037] In this application, the low-melting-point metal component is a nanoparticle, and as an example, its Dv50 can be 50-500nm.
[0038] In one optional embodiment, in S3, the oxidation treatment temperature is 100℃-200℃, and the oxidation treatment time is 2-4h.
[0039] As an example, the oxidation treatment temperature can be 100℃, 120℃, 140℃, 150℃, 170℃, 190℃, 200℃, or within any range of the above values; the oxidation treatment time can be 2h, 2.5h, 3h, 3.5h, 4h, or within any range of the above values.
[0040] Based on the above-mentioned technical means, this application limits the oxidation treatment temperature and time, and increases the temperature and holding time according to the oxidation characteristics of the metal, to ensure that the metal coating is oxidized into metal oxide, while the lithium iron phosphate particles are not oxidized.
[0041] In an optional embodiment, in S3, the sintering is segmented sintering, the segmented sintering comprising: First stage sintering: temperature 200℃-300℃, time 1-2h; Second stage sintering: temperature 350℃-450℃, time 2-3h; The third stage of sintering: the temperature is 700-850℃, and the time is 6-10h.
[0042] As an example, the sintering temperature of the first stage can be 200℃, 220℃, 240℃, 250℃, 270℃, 290℃, 300℃, or within any range of the above values; the sintering time of the first stage can be 1h, 1.2h, 1.5h, 1.8h, 2h, or within any range of the above values; the sintering temperature of the second stage can be 350℃, 370℃, 390℃, 400℃, 420℃, 440℃, 450℃, or within any range of the above values. The sintering time for the second stage can be 2h, 2.2h, 2.5h, 2.8h, 3h, or within any of the above values; the sintering temperature for the third stage can be 700℃, 730℃, 750℃, 780℃, 800℃, 820℃, 850℃, or within any of the above values; the sintering time for the third stage can be 6h, 7h, 8h, 9h, 10h, or within any of the above values.
[0043] Based on the aforementioned technical methods, segmented sintering, through low-temperature pre-sintering, allows most of the organic carbon source to decompose and undergo preliminary carbonization, while simultaneously expelling gaseous impurities, providing an excellent environment for subsequent metal coating. The second stage of sintering results in the uniform and abundant formation of fine crystal nuclei throughout the entire material system. Subsequently, at the high-temperature stage, these existing nuclei grow synchronously. This effectively suppresses the abnormal growth of a few grains, thus obtaining crystals with uniform size and perfect structure. The sintering parameters for each stage in segmented sintering are defined as follows: The first stage of sintering stabilizes after 1-2 hours based on the amount of exhaust gas during sintering; the second stage sintering temperature is when lithium iron phosphate begins to crystallize, forming uniform and abundant fine crystal nuclei; the third stage sintering enhances the crystallinity of lithium iron phosphate and the melting and growth of crystal nuclei.
[0044] In this application, the heating rate in the sintering step is conventional in the field; for example, the heating rate can be 5-10 °C / min.
[0045] In one optional embodiment, the first and second particles in the spray material are separately subjected to subsequent steps S2 and S3 to obtain large lithium iron phosphate particles and small lithium iron phosphate particles, respectively. After separating the large and small particles, they can be customized and compounded according to the application scenario. For example, different ratios can be designed for power and energy storage to achieve the required compaction density and capacity. The large particle preparation process uses two-fluid spraying to achieve surface coating of the large particles after molding, thereby improving the coating quality.
[0046] In one optional embodiment, the sintering temperature of the third stage corresponding to the first particle is 750-850℃; the sintering temperature of the third stage corresponding to the second particle is 700-750℃.
[0047] Based on the above technical means, the third sintering temperature of the first particle and the second particle are set differently, mainly because: the appearance of large particles is mainly driven by high temperature and is formed by melting small particles; small particles do not require a very high sintering temperature.
[0048] In one optional embodiment, the mass ratio of the large lithium iron phosphate particles to the small lithium iron phosphate particles is 1:9 to 9:1.
[0049] As an example, the mass ratio of the large lithium iron phosphate particles to the small lithium iron phosphate particles can be 1:9, 1:7, 1:5, 1:3, 1:1, 3:1, 5:1, 7:1, 9:1, or within any of the above values.
[0050] Based on the above-mentioned technical means, by limiting the ratio of large and small particles in lithium iron phosphate materials, the optimal balance between compaction density and rate performance can be achieved.
[0051] In an optional embodiment, in S1, the molar ratio of Li:Fe:P in the mixing and pulping step is approximately 1-1.1:0.95-1.05:0.95-1.05; In one alternative embodiment, the amount of carbon source added is 5%-30% of the mass of iron; as an example, the amount of carbon source added is 5%, 10%, 15%, 20%, 25%, 30% of the mass of iron in the iron source, or within any range of the above values.
[0052] In this application, the raw materials used in the preparation of lithium iron phosphate materials are all conventional raw materials. As an example, the lithium source includes one or more of lithium hydroxide, lithium carbonate, lithium oxalate, lithium acetate, lithium nitrate, lithium dihydrogen phosphate, and lithium citrate. The iron source includes one or more of iron phosphate, iron oxide, ferrous oxalate, iron powder, magnetite, and iron hydroxide. The carbon source includes one or more of glucose, polyvinyl alcohol, sucrose, polyethylene glycol, phenolic resin, citric acid, aniline, and vitamin C. The phosphorus source includes one or more of iron phosphate, lithium dihydrogen phosphate, phosphoric acid, ammonium dihydrogen phosphate, and ammonium monohydrogen phosphate.
[0053] In one optional embodiment, the mixing and pulping process further includes a grinding step, grinding the pulp to a particle size Dv50 of 200-400 nm; as an example, the grinding is sand milling, and the pulp particle size Dv50 is 200 nm, 220 nm, 240 nm, 250 nm, 270 nm, 290 nm, 300 nm, 330 nm, 350 nm, 370 nm, 400 nm, or within any range of the above values.
[0054] Using the aforementioned techniques, grinding the slurry to the nanoscale results in more uniform dispersion of the raw materials, which improves the crystallinity and integrity of lithium iron phosphate.
[0055] In this application, the solid content of the pulp during the mixed pulping process is 20-50 wt%.
[0056] In one optional embodiment, the spray drying is a two-fluid spray drying. Two-fluid spray drying utilizes high-speed flowing atomized gas to pull and tear the liquid material into extremely fine droplets at the top of the drying tower. Compared with traditional atomizing disc spray drying, its biggest advantage is that spray drying can form spray balls with a particle size D50 of 2-8μm. After high-temperature sintering and melting, a single spray ball can form a large lithium iron phosphate particle without further crushing. Combined with low-melting-point metal coating, the material surface can be perfectly coated in one firing.
[0057] In this application, the protective atmosphere can be a nitrogen atmosphere or an inert atmosphere (such as argon).
[0058] According to another aspect of this application, a lithium iron phosphate material is provided, which is prepared by the above-described preparation method.
[0059] According to another aspect of this application, a secondary battery is provided, comprising the aforementioned lithium iron phosphate material.
[0060] According to another aspect of this application, an electrical device is provided, including the aforementioned secondary battery.
[0061] The secondary battery and electrical equipment provided in this application have the same advantages as the aforementioned lithium iron phosphate material because they use the lithium iron phosphate material provided in this application, which will not be repeated here.
[0062] The following describes the secondary battery and electrical equipment of this application.
[0063] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.
[0064] [Positive electrode plate] The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer includes the positive active material of the first aspect of this application.
[0065] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0066] The positive electrode active material layer includes a positive electrode active material. The positive electrode active material can be selected from materials capable of absorbing and releasing lithium.
[0067] In some embodiments, the positive electrode active material layer in the positive electrode sheet of this application does not exclude other positive electrode active materials besides the lithium iron phosphate material provided in this application. For example, other positive electrode active materials may be positive electrode active materials known in the art for use in batteries. The specific type of positive electrode active material is not specifically limited and can be selected according to needs. As an example, the positive electrode active material may include, but is not limited to, ternary materials, lithium manganese phosphate (LiMnPO4), lithium cobalt phosphate (LiCoPO4), iron pyrophosphate (Li2FeP2O7), lithium cobalt oxide (LiCoO2), spinel-type lithium manganese oxide (LiMn2O4), and spinel-type lithium nickel manganese oxide (LiNi). 0.5 Mn 1.5O4), layered lithium manganate (LiMnO2), lithium nickelate (LiNiO2), lithium niobate (LiNbO2), lithium ferrite (LiFeO2), lithium manganate (LiMgO2), lithium calcium oxide (LiCaO2), lithium copper oxide (LiCuO2), lithium zinc oxide (LiZnO2), lithium molybdate (LiMoO2), lithium tantalate (LiTaO2), lithium tungstate (LiWO2), lithium nickel cobalt aluminum oxide (LiNi x Co y Al 1-x-y O2, 0 < x < 1, 0 < y < 1, 0 < x + y < 1, for example LiNi 0.8 Co 0.15 Al 0.05 O2), lithium nickel cobalt manganese oxide (LiNi x Co y Mn 1-x-y O2, 0 < x < 1, 0 < y < 1, 0 < x + y < 1, for example LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, etc.), lithium-rich materials (such as lithium-rich nickel cobalt manganese oxide), manganese dioxide (MnO2), vanadium oxides, sulfur oxides, silicate oxides, and at least one of their respective modified compounds. These materials can be used alone or in combination of two or more.
[0068] The modified compounds of the above cathode active materials can be doping modification, surface coating modification, or simultaneous doping and coating modification of the cathode active materials.
[0069] In some embodiments, the cathode current collector can be a metal foil or a composite current collector. For example, as the metal foil, aluminum foil can be used. The composite current collector can include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as substrates of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0070] In some embodiments, the positive electrode active material layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0071] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0072] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0073] [Negative electrode plate] The negative electrode includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer comprising a negative electrode active material. In some optional embodiments, the negative electrode can be directly made of a lithium-containing metal sheet. The lithium-containing metal sheet can be lithium metal or an alloy formed of lithium metal with other metals or non-metallic elements.
[0074] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0075] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0076] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0077] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0078] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0079] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0080] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0081] [Electrolytes] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0082] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0083] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0084] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0085] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0086] [Isolation membrane] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0087] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0088] In some embodiments, the electrolyte also includes additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature performance.
[0089] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0090] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.
[0091] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0092] This application does not impose any particular restrictions on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape.
[0093] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0094] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0095] In some embodiments, the aforementioned electrical device may also include a battery module or battery pack assembled from the aforementioned secondary batteries. The secondary batteries, battery modules, or battery packs can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0096] As the electrical device, a secondary battery, battery module, or battery pack can be selected according to its usage requirements. An example electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this electrical device, a battery pack or battery module can be used.
[0097] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.
[0098] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0099] Example 1 This embodiment provides a lithium iron phosphate material, the specific preparation steps and operating parameters of which are as follows: (1) Preparation of large lithium iron phosphate particles: Lithium carbonate (LiFe): iron phosphate (Fe): phosphoric acid (P): glucose (P): water was mixed with lithium carbonate (LiFe):P in a molar ratio of approximately 1:1:1. The amount of carbon source was 10% of the mass of iron. The mixture was milled to a Dv50 of 300 nm and a solid content of 30 wt%. The mixture was then spray-dried with a two-fluid to obtain a spherical precursor (first particle) with a particle size Dv50 of 5 μm. The precursor was mixed uniformly with 1 wt% nano-bismuth powder (Dv50 of 50 nm) in an argon glove box. The mixture was heated in a tube furnace under an argon atmosphere at a rate of 10 °C / min, held at 250 °C for 1 h, at 400 °C for 3 h, and at 820 °C for 8 h. The mixture was then held at 200 °C in air for 2 h to obtain large lithium iron phosphate particles.
[0100] (2) Preparation of lithium iron phosphate small particles: A slurry was prepared using the same raw materials and sand milling process as in step (1), and then spray-dried and pulverized to obtain a precursor (second particle) with a Dv50 of 600 nm. In an argon glove box, the precursor was mixed evenly with 1 wt% of nano-bismuth powder (Dv50 of 50 nm). The mixture was heated in a tube furnace under an argon atmosphere at a rate of 10 °C / min, held at 250 °C for 1 h, at 400 °C for 3 h, and at 700 °C for 8 h. Subsequently, it was held at 200 °C in an air atmosphere for 2 h, and then pulverized by air jet to obtain lithium iron phosphate small particles.
[0101] (3) Final product: Lithium iron phosphate large particles and lithium iron phosphate small particles are mechanically mixed at a mass ratio of 4:6 to obtain lithium iron phosphate material.
[0102] Example 2 This embodiment provides a lithium iron phosphate material, the specific preparation steps and operating parameters of which are as follows: (1) Preparation of large lithium iron phosphate particles: Lithium carbonate (LiFe): iron phosphate (Fe): phosphoric acid (P): glucose (Fe): P (Li:Fe:P) was mixed with water at a molar ratio of approximately 1:0.95:0.95. The amount of carbon source was 5% of the mass of iron. The mixture was milled to a Dv50 of 200 nm and a solid content of 50 wt%. The mixture was then spray-dried with a two-fluid to obtain a spherical precursor with a particle size Dv50 of 3 μm. The precursor was mixed uniformly with 0.1 wt% nano-bismuth powder (Dv50 of 50 nm) in an argon glove box. The mixture was heated in a tube furnace under an argon atmosphere at a rate of 5 °C / min, held at 300 °C for 2 h, at 450 °C for 2 h, and at 750 °C for 10 h. The mixture was then held at 100 °C in air for 4 h to obtain large lithium iron phosphate particles.
[0103] (2) Preparation of lithium iron phosphate particles: A slurry was prepared using the same raw materials and sand milling process as in step (1), and then spray-dried and pulverized to obtain a precursor with a Dv50 of 400 nm. In an argon glove box, the precursor was mixed uniformly with 0.1 wt% of nano-bismuth powder (Dv50 of 50 nm). The mixture was heated in a tube furnace under an argon atmosphere at a rate of 10 °C / min, held at 300 °C for 1 h, at 450 °C for 3 h, and at 700 °C for 10 h. Subsequently, it was held at 200 °C in an air atmosphere for 2 h, and then pulverized by air jet to obtain lithium iron phosphate particles.
[0104] (3) Final product: Lithium iron phosphate large particles and lithium iron phosphate small particles are mechanically mixed at a mass ratio of 9:1 to obtain lithium iron phosphate material.
[0105] Example 3 This embodiment provides a lithium iron phosphate material, the specific preparation steps and operating parameters of which are as follows: (1) Preparation of large lithium iron phosphate particles: Lithium carbonate (LiFe), iron phosphate (FePO4), phosphoric acid (PPO4), and glucose (GRP) were mixed with water at a Li:Fe:P molar ratio of approximately 1.1:1.05:1.05. The amount of carbon source was 30% of the mass of iron. The mixture was milled to a Dv50 of 400 nm and a solid content of 20 wt%. Spherical precursors with a particle size Dv50 of 6 μm were obtained by two-fluid spray drying. The precursors were mixed uniformly with 4 wt% nano-bismuth powder (Dv50 of 50 nm) in an argon glove box. The mixture was heated in a tube furnace under an argon atmosphere at a rate of 10 °C / min, held at 200 °C for 1 h, at 350 °C for 3 h, and at 850 °C for 6 h. The mixture was then held at 200 °C in air for 2 h to obtain large lithium iron phosphate particles.
[0106] (2) Preparation of lithium iron phosphate particles: A slurry was prepared using the same raw materials and sand milling process as in step (1), and then spray-dried and pulverized to obtain a precursor with a Dv50 of 1000 nm. In an argon glove box, the precursor was mixed uniformly with 4 wt% nano-bismuth powder (Dv50 of 50 nm). The mixture was heated in a tube furnace under an argon atmosphere at a rate of 5 °C / min, held at 200 °C for 2 h, at 350 °C for 2 h, and at 750 °C for 6 h. Subsequently, it was held at 100 °C in an air atmosphere for 4 h, and then pulverized by air jet to obtain lithium iron phosphate particles.
[0107] (3) Final product: Lithium iron phosphate large particles and lithium iron phosphate small particles are mechanically mixed at a mass ratio of 1:9 to obtain lithium iron phosphate material.
[0108] Example 4 This embodiment provides a lithium iron phosphate material, the specific preparation steps and operating parameters of which are as follows: (1) Preparation of large lithium iron phosphate particles: Lithium carbonate (LiFe): iron phosphate (Fe): phosphoric acid (P): glucose (P): water was mixed with lithium carbonate (LiFe):P at a molar ratio of approximately 1.05:1:1. The amount of carbon source was 18% by mass of iron. The mixture was milled to a Dv50 of 300 nm and a solid content of 35 wt%. The mixture was then spray-dried with a two-fluid to obtain a spherical precursor with a particle size Dv50 of 4.5 μm. The precursor was mixed uniformly with 2 wt% nano-bismuth powder (Dv50 of 50 nm) in an argon glove box. The mixture was heated in a tube furnace under an argon atmosphere at a rate of 8 °C / min, held at 250 °C for 1.5 h, at 400 °C for 2.5 h, and at 820 °C for 8 h. The mixture was then held at 150 °C in air for 3 h to obtain large lithium iron phosphate particles.
[0109] (2) Preparation of lithium iron phosphate particles: A slurry was prepared using the same raw materials and sand milling process as in step (1), and then spray-dried and pulverized to obtain a precursor with a Dv50 of 700 nm. In an argon glove box, the precursor was mixed uniformly with 2 wt% nano-bismuth powder (Dv50 of 50 nm). The mixture was heated in a tube furnace under an argon atmosphere at a rate of 7 °C / min, held at 250 °C for 1.5 h, at 400 °C for 2.5 h, and at 730 °C for 8 h. Subsequently, it was held at 150 °C in an air atmosphere for 3 h, and then pulverized by air jet to obtain lithium iron phosphate particles.
[0110] (3) Final product: Lithium iron phosphate large particles and lithium iron phosphate small particles are mechanically mixed at a mass ratio of 1:1 to obtain lithium iron phosphate material.
[0111] Example 5 This embodiment provides a lithium iron phosphate material, the specific preparation steps and operating parameters of which are as follows: (1) Preparation of large lithium iron phosphate particles: Lithium hydroxide (LiPO), ferric oxide (FeO), ammonium hydrogen phosphate (MPH), and sucrose (SPH) were mixed with water at a Li:Fe:P molar ratio of approximately 1.05:1:1. The amount of carbon source was 18% of the mass of iron. The mixture was milled to a Dv50 of 300 nm and a solid content of 35 wt%. Spherical precursors with a particle size Dv50 of 5.5 μm were obtained by two-fluid spray drying. The precursors were mixed uniformly with 2 wt% nano-bismuth powder (Dv50 of 50 nm) in an argon glove box. The mixture was heated in a tube furnace under an argon atmosphere at a rate of 8 °C / min, held at 250 °C for 1.5 h, at 400 °C for 2.5 h, and at 820 °C for 8 h. The mixture was then held at 170 °C in air for 3 h to obtain large lithium iron phosphate particles.
[0112] (2) Preparation of lithium iron phosphate particles: A slurry was prepared using the same raw materials and sand milling process as in step (1), and then spray-dried and pulverized to obtain a precursor with a Dv50 of 850 nm. In an argon glove box, the precursor was mixed uniformly with 2 wt% nano-bismuth powder (Dv50 of 50 nm). The mixture was heated in a tube furnace under an argon atmosphere at a rate of 7 °C / min, held at 250 °C for 1.5 h, at 400 °C for 2.5 h, and at 730 °C for 8 h. Subsequently, it was held at 130 °C in an air atmosphere for 3 h, and then pulverized by air jet to obtain lithium iron phosphate particles.
[0113] (3) Final product: Lithium iron phosphate large particles and lithium iron phosphate small particles are mechanically mixed at a mass ratio of 1:1 to obtain lithium iron phosphate material.
[0114] Example 6 This embodiment provides a lithium iron phosphate material, the specific preparation steps and operating parameters of which are as follows: (1) Preparation of large lithium iron phosphate particles: Lithium carbonate (LiFe): iron ferrous oxalate (FeO): phosphoric acid (P): polyvinyl alcohol (PE) (Li:Fe:P) was mixed with water in a molar ratio of approximately 1.05:1:1. The amount of carbon source was 18% of the mass of iron. The mixture was milled to a Dv50 of 300 nm and a solid content of 35 wt%. Spherical precursors with a particle size Dv50 of 5.5 μm were obtained by two-fluid spray drying. The precursors were mixed uniformly with 2 wt% nano-bismuth powder (Dv50 of 50 nm) in an argon glove box. The mixture was heated in a tube furnace under an argon atmosphere at a rate of 8 °C / min, held at 250 °C for 1.5 h, at 400 °C for 2.5 h, and at 820 °C for 8 h. The mixture was then held at 170 °C in air for 3 h to obtain large lithium iron phosphate particles.
[0115] (2) Preparation of lithium iron phosphate particles: A slurry was prepared using the same raw materials and sand milling process as in step (1), and then spray-dried and pulverized to obtain a precursor with a Dv50 of 850 nm. In an argon glove box, the precursor was mixed uniformly with 2 wt% nano-bismuth powder (Dv50 of 50 nm). The mixture was heated in a tube furnace under an argon atmosphere at a rate of 7 °C / min, held at 250 °C for 1.5 h, at 400 °C for 2.5 h, and at 730 °C for 8 h. Subsequently, it was held at 130 °C in an air atmosphere for 3 h, and then pulverized by air jet to obtain lithium iron phosphate particles.
[0116] (3) Final product: Lithium iron phosphate large particles and lithium iron phosphate small particles are mechanically mixed at a mass ratio of 1:1 to obtain lithium iron phosphate material.
[0117] Example 7 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that an equal amount of tin (Dv50 is 100nm) is used instead of nano bismuth powder.
[0118] Example 8 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that an equal amount of antimony-tin alloy (specifically, the composition is 8% antimony by mass, 92% tin by mass, and Dv50 of 80nm) is used instead of nano-bismuth powder.
[0119] Example 9 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that the mass ratio of large lithium iron phosphate particles to small lithium iron phosphate particles is 1:3.
[0120] Example 10 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that the mass ratio of large lithium iron phosphate particles to small lithium iron phosphate particles is 1:5.
[0121] Example 11 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that the mass ratio of large lithium iron phosphate particles to small lithium iron phosphate particles is 3:1.
[0122] Example 12 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that the mass ratio of large lithium iron phosphate particles to small lithium iron phosphate particles is 5:1.
[0123] Example 13 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that: the first particle and the second particle simultaneously undergo subsequent steps S2 and S3, as detailed below: A slurry was prepared using the same raw materials and milling process as in Example 1. After spray drying and pulverization, precursors with a Dv50 of 5 micrometers (first particle) and a Dv50 of 600 nm (second particle) were obtained. In an argon-filled glove box, the precursors (first particle to second particle mass ratio of 4:6) were mixed uniformly with 1 wt% nano-bismuth powder (Dv50 of 50 nm). The mixture was then heated in a tube furnace under an argon atmosphere at a rate of 10 °C / min, held at 250 °C for 1 h, at 400 °C for 3 h, and at 750 °C for 8 h. Subsequently, it was held at 200 °C in air for 2 h, and then pulverized by air jet milling to obtain lithium iron phosphate material.
[0124] Example 14 This embodiment provides a lithium iron phosphate material, which differs from Embodiment 1 in that it uses one-step sintering instead of segmented sintering, as detailed below: In step (1), the mixture is heated in a tube furnace at 10°C / min under an argon atmosphere and held at 820°C for 8 hours. Then it is held at 200°C in an air atmosphere for 2 hours to obtain large lithium iron phosphate particles.
[0125] In step (2), the mixture is heated in a tube furnace at 10°C / min under an argon atmosphere and held at 700°C for 8 hours. Then it is held at 200°C in an air atmosphere for 2 hours and then pulverized by airflow to obtain lithium iron phosphate particles.
[0126] All other operations are the same as in Example 1.
[0127] Comparative Example 1 This comparative example provides a lithium iron phosphate material, which differs from Example 1 in that: no low-melting-point metal components are added in steps (1) and (2).
[0128] Comparative Example 2 This comparative example provides a lithium iron phosphate material, which differs from Example 1 in that tungsten is used instead of low-melting-point metal components in steps (1) and (2).
[0129] Comparative Example 3 This comparative example provides a lithium iron phosphate material, which differs from Example 1 in that: the particle size Dv50 of the first particle in step (1) is 7 μm; and the particle size Dv50 of the first particle in step (2) is 300 nm.
[0130] Comparative Example 4 This comparative example provides a lithium iron phosphate material, which differs from Example 1 in that: the particle size Dv50 of the first particle in step (1) is 2 μm; and the particle size Dv50 of the first particle in step (2) is 1500 nm.
[0131] Comparative Example 5 This comparative example provides a lithium iron phosphate material, which differs from Example 1 in that the coating timing is different. Specifically, after the large / small particles are sintered once, the sintered material and low-melting-point metal powder are mixed and sintered separately, and finally the large and small particles are compounded. The specific operation is as follows: (1) Preparation of large lithium iron phosphate particles: Lithium carbonate (LiFe), iron phosphate (FeP), phosphoric acid (POP), and glucose (GRP) were mixed with water in a Li:Fe:P molar ratio of approximately 1:1:1. The amount of carbon source was 10% of the mass of iron. The mixture was milled to a Dv50 of 300 nm and a solid content of 30 wt%. The mixture was then spray-dried with a two-fluid to obtain a spherical precursor (first particle) with a particle size Dv50 of 5 μm. The material was heated in a tube furnace under an argon atmosphere at a rate of 10 °C / min, held at 250 °C for 1 h, held at 400 °C for 3 h, and held at 820 °C for 8 h to obtain a first calcined material A. In an argon glove box, the first calcined material A was mixed evenly with 1 wt% of nano-bismuth powder (Dv50 of 50 nm). The mixture was heated to 700 °C at a rate of 10 °C / min under an argon atmosphere and held for 5 h. Then, it was held at 200 °C in an air atmosphere for 2 h to obtain coated large lithium iron phosphate particles A.
[0132] (2) Preparation of lithium iron phosphate small particles: The same raw materials and sand milling process as in step (1) were used to prepare the slurry. After spray drying and pulverization, a precursor (second particle) with a Dv50 of 600 nm was obtained. The material was heated in a tube furnace under an argon atmosphere at 10 °C / min, held at 250 °C for 1 h, held at 400 °C for 3 h, and held at 700 °C for 8 h to obtain a calcined material B. In an argon glove box, the calcined material B was mixed evenly with 1 wt% of nano bismuth powder (Dv50 of 50 nm). Under an argon atmosphere, the temperature was increased to 700 °C at 10 °C / min and held for 5 h. Then, it was held at 200 °C in an air atmosphere for 2 h to obtain coated lithium iron phosphate small particles B.
[0133] Final product: Lithium iron phosphate large particles A and lithium iron phosphate small particles B are mechanically mixed at a mass ratio of 4:6 to obtain lithium iron phosphate material.
[0134] Experimental Example 1. Compacted density: Refer to GB / T30835-2014 to test the compaction of 3T powder. Test instrument: electronic powder compaction tester, Shenzhen Sansi Zongheng UTM7305.
[0135] 2. Electrical performance testing The lithium iron phosphate materials provided in the various embodiments and comparative examples were used to prepare coin cells for performance testing, as detailed below: Fabrication of button cells: 2.1 Preparation of the positive electrode sheet Aluminum foil with a thickness of 13μm was used as the positive electrode current collector.
[0136] Lithium iron phosphate material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are thoroughly mixed in an appropriate amount of solvent NMP at a weight ratio of 97.5:1.4:1.1 to form a uniform positive electrode slurry. The positive electrode slurry is uniformly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0137] 2.2 Preparation of the negative electrode sheet A copper foil with a thickness of 8μm was used as the negative electrode current collector.
[0138] The negative electrode active material graphite, the binder styrene-butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC-Na), and the conductive agent carbon black (SuperP) are mixed in an appropriate amount of deionized water at a weight ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry. The negative electrode slurry is then uniformly coated onto the surface of the negative electrode current collector copper foil. After drying and cold pressing, the negative electrode sheet is obtained.
[0139] 2.3 Separating membrane Porous polyethylene (PE) membrane is used as the separator.
[0140] 2.4 Preparation of Electrolyte Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent. Then, fully dried LiPF6 was dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0141] 2.5 Preparation of Secondary Batteries The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. The electrode assembly is then wound up. The electrode assembly is placed in an outer packaging shell, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.
[0142] 2.6 Cyclic performance test of secondary batteries at 45℃ Under a constant temperature environment of 45℃, the secondary battery is charged at 1C to 3.65V, and then charged at a constant voltage of 3.65V until the current is less than or equal to 0.05C. After resting for 5 minutes, it is discharged at 1C to 2.5V, and the discharge capacity at this point is recorded as E0. The aforementioned charge-discharge cycle is repeated until the discharge capacity decreases to 80% of E0. The number of cycles completed by the secondary battery at this point is recorded.
[0143] 2.7 Rate performance test of secondary batteries at 25℃ Under a constant temperature environment of 25℃, the secondary battery was activated once, charged at 0.1C to 3.65V, and then charged at 3.65V with a constant voltage until the current was less than or equal to 0.05C. It was then allowed to stand for 5 minutes, and then discharged at 0.1C to 2.5V. This process was then repeated at different charging rates: 0.2C, 0.5C, 1C, 2C, 5C, and 10C, with a discharge rate of 0.1C, yielding different discharge capacities.
[0144] The specific test results are shown in the table below: Table 1
[0145] As shown in the test results in the table above, the method for preparing lithium iron phosphate material provided in this application utilizes the melting, wetting, and subsequent oxidation behavior of low-melting-point metal components under specific conditions to construct a dense and uniform nanoscale oxide protective layer. This effectively improves the electronic conductivity and structural stability of the material. Through the gradation of large and small particles, the lithium iron phosphate material possesses both high compaction density and excellent high-rate charge-discharge performance and cycle performance. Further improvements in these properties can be achieved by separately processing the low-melting-point metal components, stepwise sintering, and large and small particles.
[0146] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this application.
Claims
1. A method for preparing lithium iron phosphate material, characterized in that, Includes the following steps: S1, mix lithium source, iron source, phosphorus source and carbon source to form a slurry, spray dry to obtain spray material, the spray material includes first particles with a particle size Dv50 of 3-6μm and second particles with a particle size Dv50 of 400-1000nm; S2, Under a protective atmosphere, the spray material is mixed with a low-melting-point metal component to obtain a mixture; wherein the melting point of the low-melting-point metal component is 150-700℃; S3, the mixture is sintered under a protective atmosphere and oxidized in an oxygen-containing atmosphere to obtain the lithium iron phosphate material.
2. The method for preparing lithium iron phosphate material according to claim 1, characterized in that, In S2, the amount of the low-melting-point metal component accounts for 0.1%-4% of the mass of the spray material; And / or, the low-melting-point metal component includes at least one of elemental aluminum, zinc, magnesium, bismuth, lead, tin, cadmium, indium, and alloys containing the above elements; Optionally, the low-melting-point metal component includes at least one of elemental bismuth, elemental tin, tin alloys, aluminum alloys, zinc alloys, and magnesium alloys.
3. The method for preparing lithium iron phosphate material according to claim 1, characterized in that, In S3, the oxidation treatment is carried out at a temperature of 100-200℃ for 2-4 hours.
4. The method for preparing lithium iron phosphate material according to claim 1, characterized in that, In S3, the sintering is segmented sintering, and the segmented sintering includes: First stage sintering: temperature 200-300℃, time 1-2h; Second stage sintering: temperature 350-450℃, time 2-3h; The third stage of sintering: the temperature is 700-850℃, and the time is 6-10h.
5. The method for preparing lithium iron phosphate material according to claim 4, characterized in that, The first and second particles in the spray material are separated and subjected to subsequent steps S2 and S3 to obtain large lithium iron phosphate particles and small lithium iron phosphate particles respectively. Optionally, the sintering temperature of the third stage corresponding to the first particle is 750-850℃; the sintering temperature of the third stage corresponding to the second particle is 700-750℃.
6. The method for preparing lithium iron phosphate material according to claim 5, characterized in that, The mass ratio of large lithium iron phosphate particles to small lithium iron phosphate particles is 1:9 to 9:
1.
7. The method for preparing lithium iron phosphate material according to claim 1, characterized in that, In S1, during the mixing and pulping step, the molar ratio of Li:Fe:P is 1-1.1:0.95-1.05:0.95-1.05; And / or, the amount of carbon source added is 5%-30% of the mass of iron; And / or, the mixing and pulping process further includes a grinding step, grinding the pulp until the particle size Dv50 is 200-400 nm; And / or, the spray drying is a two-fluid spray drying.
8. A lithium iron phosphate material, characterized in that, It is prepared by the preparation method according to any one of claims 1-7.
9. A secondary battery, characterized in that, Including the lithium iron phosphate material as described in claim 8.
10. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 9.
Citation Information
Cited By
Battery monomer and preparation method thereof, battery device, power utilization device and energy storage device
CN122025733A