A polymer tackifier, its preparation and use

By combining polymer thickeners with modified starch and hydrolyzed polyacrylonitrile ammonium salt, a stable drilling fluid system was formed, which solved the rheological and filtration problems of drilling fluid in high salinity environments and achieved performance optimization of drilling fluid in high-salt and high-calcium environments.

CN121343060BActive Publication Date: 2026-11-10QINGDAO INST OF SURVEYING & MAPPING SURVEY +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202511540524.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-10-27
Publication Date
2026-11-10
Estimated Expiration
2045-10-27

AI Technical Summary

Technical Problem

Existing drilling fluids are not strong enough to resist calcium ions in high-salinity environments, and traditional treatment agents have poor temperature and salt resistance, making it difficult to meet the drilling needs of complex formations.

Method used

A polymer thickener is prepared by polymerization reaction of specific monomers and crosslinking agents, and then combined with bentonite, modified starch and hydrolyzed polyacrylonitrile ammonium salt to form a drilling fluid resistant to brine intrusion. The hydroxyl and quaternary ammonium salt groups enhance the steric hindrance and electrostatic adsorption between clay particles in a high-salt environment, forming a stable drilling fluid system.

Benefits of technology

In high-salinity environments, polymer thickeners significantly improve the rheological properties and filtration loss reduction of drilling fluids, and can resist 33% NaCl and 15% CaCl2, meeting the drilling operation requirements in high-salinity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121343060B_ABST
    Figure CN121343060B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of compounds, and relates to a polymer tackifier as well as a preparation method and application thereof. The polymer tackifier is generated through water bath constant-temperature heating reaction of 2-acrylamido-2-methylpropanesulfonic acid, acrylamide and sulfonic acid with water as a continuous phase under the action of a crosslinking agent N,N-methylenebisacrylamide and an initiator ammonium persulfate. The anti-halogen water invasion drilling fluid of the application can still maintain good rheological property and stability in a high-salt and high-calcium environment, can resist 33% NaCl and 15% CaCl2, and can be applied to a high-mineralization complex stratum environment. The polymer tackifier is used for preparing a drilling fluid. The anti-halogen water invasion drilling fluid comprises 40 parts of bentonite, 2 parts of sodium hydroxide, 10-20 parts of the polymer tackifier, 15 parts of modified starch, 15 parts of hydrolyzed polyacrylonitrile ammonium salt and 1000 parts of water. The anti-halogen water invasion drilling fluid of the application can still maintain good rheological property and stability in a high-salt and high-calcium environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of compound technology and relates to a polymer tackifier, its preparation method, and its uses. Background Technology

[0002] In deep geological exploration, drilling often encounters formations with high concentrations of brine. Large amounts of salt, calcium, and other substances can infiltrate or dissolve into the drilling fluid, causing problems such as deterioration of the drilling fluid's rheological properties and increased filtration loss. In severe cases, this can lead to lost circulation, overflows, and stuck pipe. Specifically, in some areas, the formation water is highly mineralized and rich in metal cations such as Ca²⁺ and Mg²⁺. These cations can infiltrate the drilling fluid and undergo ion exchange with the bentonite in the fluid, adversely affecting the viscosity and filtration loss reduction performance of conventional drilling fluids, significantly limiting the efficiency and quality of drilling operations.

[0003] Currently, traditional treatment agents are mainly used in the field. While traditional natural polymers (such as carboxymethyl cellulose and polyacrylamide) are low-cost and environmentally friendly, their temperature and salt resistance is insufficient. Domestic and international research on temperature and salt resistant treatment agents mainly focuses on monomer structure design and copolymer modification. Compared to ternary copolymers, the synthesis of quaternary or pentadienyl copolymers often introduces more temperature and salt resistant groups, increasing production costs and complicating the synthesis process. Although modified polymers exhibit good temperature and salt resistance, most have high biotoxicity and poor environmental performance. Furthermore, commonly used water-based drilling fluid systems, primarily based on polysulfonate drilling fluids, generally have calcium ion resistance levels not exceeding 1000 ppm, resulting in insufficient resistance to calcium-containing salt deposits. Research on drilling fluid systems suitable for high-saltification environments is also limited.

[0004] Chinese invention patent CN 112048289 A discloses a high-salinity water-based drilling fluid, comprising the following raw material components in parts by weight: 4-6 parts organic bentonite; 2-4 parts modified asphalt; 0.8-1.5 parts salt-resistant copolymer; 0.5-1.5 parts hydrolyzed polyacrylonitrile potassium salt; 2-3 parts sulfonated lignite resin; 1-4 parts plugging agent while drilling; 0.2-0.5 parts coating agent; 0.5-1 part defoamer; 0.3-0.5 parts sodium carbonate; 0.8-1 parts sodium hydroxide; and 95-105 parts brine. This drilling fluid exhibits good colloidal stability, strong resistance to salt intrusion, strong inhibition, good rheological properties, and excellent suspension and rock powder carrying capacity, meeting operational requirements. However, this patent uses a large amount of treatment agents, and the viscosity-increasing and filtration loss-reducing effects are not significant. Chinese invention patent CN 115991978 A discloses a high-calcium-resistant ultra-high-density drilling fluid system and its preparation method. The drilling fluid system has a temperature resistance of up to 165℃, a calcium ion resistance of 13000 mg / L, and a maximum density of 2.55 g / cm³. 3However, the system's resistance to calcium ions and its ability to achieve high mineralization still fall short, making it difficult to meet the drilling requirements of complex formations.

[0005] Therefore, how to effectively select and optimize additives to improve the performance of drilling fluid systems in high-salinity environments remains a current research hotspot. Summary of the Invention

[0006] To address the problems existing in the background art, the present invention provides a polymer thickener and its preparation method, and also provides the use of the polymer thickener in the preparation of brine-resistant drilling fluids. The technical solution adopted by this invention to solve its technical problem is as follows: In a first aspect, the present invention provides a polymeric tackifier having the following structural formula: ; The values ​​of x, y, and z are (60-70), (15-20), and (15-20), respectively.

[0007] Furthermore, the present invention also provides a method for preparing the polymer thickener, comprising: S1, adding 250 parts by weight of deionized water to a beaker, adding 8 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid while stirring, stirring for 10 min, adjusting the pH value of the system to 7-8, and stirring evenly to obtain mixture 1; S2. Under stirring conditions, add 8 parts by weight of acrylamide and 5 parts by weight of sulfonic acid to mixture 1, then add 0.02~0.1 parts by weight of crosslinking agent, and stir for 10~20 min to obtain mixture 2. S3. Transfer mixture 2 to the reactor, and under stirring conditions, purge with nitrogen to remove oxygen for 30 minutes, then raise the temperature and maintain it at 60°C. At 3℃, 0.1~0.3 parts by weight of initiator were dissolved in 5 parts by weight of water and added to the reactor. The polymerization reaction was carried out by continuous stirring for 4~5 hours to obtain mixture 3. S4. After the reaction is complete, stop heating and cool. Then, repeatedly soak and wash the product with detergent 3-5 times to obtain mixture 4. S5. Place the mixture 4 in an oven for 24~30 hours at a temperature of 45~60℃. After drying, remove it and crush it to obtain the polymer thickener product powder.

[0008] Preferably, the sulfonic acid is selected from one or more of sodium methpropylene sulfonate, sodium vinyl sulfonate, and sodium allyl sulfonate.

[0009] Preferably, the crosslinking agent is N,N'-methylenebis(propylene)vinylamide.

[0010] Preferably, the initiator is ammonium persulfate.

[0011] Furthermore, the present invention also provides the use of the polymer thickener, which can be used to prepare brine-resistant drilling fluids.

[0012] Furthermore, the present invention also provides a drilling fluid resistant to brine intrusion, comprising the following raw materials in parts by weight: 40 parts bentonite, 2 parts sodium hydroxide, 10-20 parts polymer thickener, 15 parts modified starch, 15 parts hydrolyzed polyacrylonitrile ammonium salt, and 1000 parts water.

[0013] Furthermore, the present invention also provides a method for preparing the brine-resistant drilling fluid, comprising the following steps: S1. First, mix 1000 parts water with 40 parts bentonite, stir thoroughly for 20 minutes at 10000 r / min, and then cure at room temperature for 24 hours to form mixture 1. S2. Under stirring conditions of 8000~10000r / min, slowly and evenly add 10~20 parts of polymer thickener to mixture 1, stir for 15min until uniform, then add 10~20 parts of high-efficiency salt-resistant filtration loss-reducing modified starch and 10~20 parts of hydrolyzed polyacrylonitrile ammonium salt in sequence, stir for 20min to form mixture 2. S3. Add NaOH to adjust the pH value of mixture 2, and stir thoroughly for 10 minutes at 1000 r / min to obtain the brine-resistant drilling fluid.

[0014] The beneficial effects of this invention are: 1. The preparation process of the polymer thickener and drilling fluid provided by the present invention is simple, easy to operate, and suitable for large-scale industrial production.

[0015] 2. The brine-resistant drilling fluid of the present invention possesses stable rheological properties and reduced filtration loss performance. The modified starch in the brine-resistant drilling fluid system enhances the steric hindrance effect between clay particles through the hydration film formed by hydroxyl groups. Its salting-out effect promotes its aggregation in the filter cake pores, forming a tight-fitting plugging layer. The hydrolyzed polyacrylonitrile ammonium salt contains carboxylic acid, carboxyamium, amide, and imine groups, possessing salt resistance properties. The quaternary ammonium salt (-NH4⁺) is electrostatically adsorbed onto the surface of clay or solid particles, reducing electrostatic repulsion between particles and improving flow pattern stability. In high-salt environments, the carboxylic acid and ammonium (NH4⁺) groups can complex with high-valence ions such as Na⁺ / Ca²⁺ to form soluble complexes, preventing the formation of salt deposits and suppressing salt sensitivity effects. This allows the drilling fluid system to maintain good filtration loss reduction even in high-salt brine environments. The three materials form a stable drilling fluid system through charge complementarity, molecular chain entanglement, and multi-element plugging, which inhibits the damage of salt / calcium to clay, thereby maintaining the stability of viscosity and filtration loss, and ultimately achieving synergistic optimization of the rheological-filtration performance of drilling fluid in brine-infiltrated environments.

[0016] 3. The anti-brine drilling fluid system of the present invention has good resistance to NaCl and CaCl2, and can resist 33% NaCl and 15% CaCl2, which can meet the requirements of drilling operations in high-mineralization environments. Attached Figure Description

[0017] Figure 1 This is the equation for the polymerization reaction during the preparation of the polymer tackifier in this invention; Figure 2 The images show the mud cake effect and SEM image of the brine-resistant drilling fluid prepared according to this invention in fresh water-based slurry and 15% calcium water slurry. Detailed Implementation

[0018] In the following description of the present invention, the term "parts" refers to "parts by weight" unless otherwise specified, and "water" is "deionized water" unless otherwise specified in the preparation of the polymer thickener. Tap water can be used in the preparation of drilling fluid.

[0019] The principles and features of the present invention are described below with reference to specific embodiments. The described embodiments are only some embodiments of this disclosure, and not all embodiments. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention.

[0020] Example 1: A polymer tackifier with the following structural formula: ; The ranges of x, y, and z are (60-70), (15-20), and (15-20), respectively.

[0021] The polymer tackifier is prepared from the following raw materials in parts by weight: 8 parts of 2-acrylamido-2-methylpropanesulfonic acid, 8 parts of acrylamide, 5 parts of sodium allyl sulfonate, 0.02 parts of crosslinking agent N,N'-methylenebispropylene vinylamide, 0.1 parts of initiator ammonium persulfate, and 250 parts of water. The preparation method of the above-mentioned polymer tackifier includes the following steps: 1. Add deionized water to a beaker, and add 2-acrylamido-2-methylpropanesulfonic acid while stirring at 1200 r / min. Stir for 10 min, adjust the pH of the system to 7-8 with sodium hydroxide solution, and stir evenly to obtain mixture 1. 2. Add acrylamide and sulfonic acid to mixture 1 at 1200 r / min, then add crosslinking agent N,N'-methylenebispropylene vinylamide, and stir for 10~20 min to obtain mixture 2; 3. Transfer mixture 2 to the reactor, stir at 1200 rpm, purge with nitrogen for 30 minutes to remove oxygen, then raise the temperature and maintain it at 60°C. At 3℃, ammonium persulfate dissolved in 5 parts by weight of water was added to the reactor as an initiator, and the polymerization reaction was carried out with continuous stirring for 4-5 hours to obtain mixture 3; the polymerization reaction equation is as follows. Figure 1 As shown.

[0022] 4. After the reaction is complete, stop heating and cool. Then wash the product repeatedly with detergent ethanol 3-5 times to obtain mixture 4. 5. Place the mixture 4 in an oven for 24-30 hours at a temperature of 45-60℃. After drying, remove it and crush it to obtain polymer thickener A1.

[0023] Example 2: A polymer tackifier prepared from the following raw materials in parts by weight: 9 parts 2-acrylamido-2-methylpropanesulfonic acid, 11 parts acrylamide, 5 parts sodium p-styrenesulfonate, 0.1 parts crosslinking agent N,N'-methylenebispropylene vinylamide, 0.02 parts initiator ammonium persulfate, and 100 parts water. The preparation method of the above polymer tackifier is as described in Example 1, and polymer tackifier A2 is obtained.

[0024] Example 3 A polymer tackifier was prepared from the following raw materials in parts by weight: 9 parts of 2-acrylamido-2-methylpropanesulfonic acid, 11 parts of acrylamide, 4 parts of sodium methacrylate sulfonate, 0.1 parts of crosslinking agent N,N'-methylenebispropylene vinylamide, 0.02 parts of initiator ammonium persulfate, and 100 parts of water. The preparation method of the above polymer tackifier is as described in Example 1, and polymer tackifier A3 is obtained.

[0025] Comparative Example 1: A polymer tackifier as described in Example 1, except that: 7 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7 parts of sodium allyl sulfonate, and 6 parts of acrylamide are added; the composition of other raw materials is the same as in Example 1.

[0026] The preparation method of the above polymer tackifier is as described in Example 1, and polymer tackifier B1 is obtained.

[0027] Comparative Example 2: A commonly used traditional thickener, high-viscosity cellulose, sourced from Pingxiang Huixin Drilling Materials Factory, was added in the amount of 2 parts.

[0028] The performance of the polymer tackifier provided by this invention was compared and evaluated: I. Performance Evaluation of Freshwater Slurry Freshwater-based slurry: Take 350mL of distilled water, add 14.0g of sodium bentonite and 0.2g of anhydrous sodium carbonate, stir at high speed for 20min, and cure in a sealed container at 25±1℃ for 24h to obtain freshwater-based slurry.

[0029] Add 3.5g of freshwater-based slurry to the sample and stir at high speed for 20 minutes. Then, at 25±1℃, test the filtration loss and apparent viscosity of Comparative Examples 1 and 2, and Examples 1 to 3 according to the provisions of GB / T 16783.1-2014.

[0030] The filtration loss and apparent viscosity of each sample in freshwater-based slurry are compared in Table 1.

[0031] Table 1 Comparison of filtrate loss and apparent viscosity of samples in freshwater-based slurry

[0032] As can be seen from Table 1, in freshwater-based slurry, under the same dosage, the polymer thickeners used in this invention have better thickening effects than commonly used traditional thickeners. Moreover, the polymer thickeners used in this invention also show better filtration loss reduction effects after addition.

[0033] II. Performance Evaluation of 4% Salt Water Slurry Take 350 mL of distilled water, add 14.0 g of sodium bentonite and 0.2 g of anhydrous sodium carbonate, stir at high speed for 20 min, and cure in a sealed container at 25 ± 1 °C for 24 h to obtain the base slurry.

[0034] Take the base slurry, add 7g of sample, add 4% sodium chloride, stir at high speed for 20min to obtain 4% brine slurry, and then test the filtration loss and apparent viscosity of Comparative Examples 1 and 2, and Examples 1 to 3 at 25±1℃ according to the provisions of GB / T 16783.1-2014.

[0035] The comparison of filtration loss of each sample in 4% saline slurry is shown in Table 2.

[0036] Table 2 Comparison of Filtration Loss of Samples in 4% Brine Slurry .

[0037] As can be seen from Table 2, in 4% brine slurry, under the same dosage, the polymer thickener used in this invention has a better thickening effect than commonly used traditional thickeners, and the filtration loss reduction effect is obvious compared with 4% brine slurry, indicating that the polymer thickener of this invention has better salt resistance.

[0038] III. Performance Evaluation of 0.5% Calcium Water Slurry Take 350 mL of distilled water, add 14.0 g of sodium bentonite and 0.2 g of anhydrous sodium carbonate, stir at high speed for 20 min, and cure in a sealed container at 25 ± 1 °C for 24 h to obtain the base slurry.

[0039] Take the base slurry, add 7g of sample, add 0.5% sodium chloride, stir at high speed for 20min to obtain 0.5% brine slurry, and then test the filtration loss and apparent viscosity of Comparative Examples 1 and 2, and Examples 1 to 3 at 25±1℃ according to the provisions of GB / T 16783.1-2014.

[0040] The comparison of filtration loss of each sample in 0.5% calcium slurry is shown in Table 3.

[0041] Table 3 Comparison of filtration loss of samples in 0.5% calcium slurry .

[0042] As can be seen from Table 3, in 0.5% calcium slurry, under the same dosage, the polymer thickener used in this invention has a better thickening effect than commonly used traditional thickeners, and compared with 4% brine slurry, the filtration loss reduction effect is obvious, indicating that the polymer thickener of this invention has better anti-calcium properties.

[0043] In the example samples, due to different monomer designs, the properties of the synthesized polymers also differed. In summary, it can be seen that the polymer thickeners prepared in the examples of this invention possess excellent thickening properties and resistance to salt and calcium. Comparatively, the performance of Example 1 is significantly superior to other prepared thickeners. Therefore, the polymer thickener prepared in Example 1 is selected in this invention for subsequent preparation of a brine-resistant drilling fluid system.

[0044] Example 4: A drilling fluid resistant to brine intrusion is prepared from the following raw materials in parts by weight: 40 parts bentonite, 2 parts sodium hydroxide, 10 parts polymer thickener, 15 parts modified starch, 15 parts hydrolyzed polyacrylonitrile ammonium salt, 100 parts sodium chloride, and 1000 parts water.

[0045] The preparation method of the above-mentioned anti-brine drilling fluid includes the following steps: 1. First, mix water and bentonite, stir thoroughly at 10000r / min for 20 minutes, and then cure at room temperature for 24 hours to form mixture 1; 2. Under stirring conditions of 8000~10000r / min, slowly and evenly add polymer thickener to mixture 1, stir for 15min until uniform, then add modified starch and hydrolyzed polyacrylonitrile ammonium salt in sequence, stir for 20min to form mixture 2. 3. Add NaOH to adjust the pH value of mixture 2, and stir thoroughly for 10 minutes at 1000 r / min to obtain brine-resistant drilling fluid C1.

[0046] Example 5: A drilling fluid resistant to brine intrusion is prepared from the following raw materials in parts by weight: 40 parts bentonite, 2 parts sodium hydroxide, 15 parts polymer thickener, 15 parts modified starch, 15 parts hydrolyzed polyacrylonitrile ammonium salt, 100 parts sodium chloride, and 1000 parts water.

[0047] The above-mentioned method for preparing the anti-brine drilling fluid is as described in Example 4, resulting in anti-brine drilling fluid C2.

[0048] Example 6: A drilling fluid resistant to brine intrusion is prepared from the following raw materials in parts by weight: 40 parts bentonite, 2 parts sodium hydroxide, 20 parts polymer thickener, 15 parts modified starch, 15 parts hydrolyzed polyacrylonitrile ammonium salt, 100 parts sodium chloride, and 1000 parts water.

[0049] The above-mentioned method for preparing the anti-brine drilling fluid is as described in Example 4, resulting in anti-brine drilling fluid C3.

[0050] Comparative Example 3 is a drilling fluid that differs from Example 4 in that it does not contain the three treatment agents: polymer thickener, modified starch, and hydrolyzed polyacrylonitrile ammonium salt. The other raw material composition and preparation method are the same.

[0051] Comparative Example 4 is a drilling fluid that differs from Example 4 in that it does not contain a polymer thickener, but the other raw material composition and preparation method are the same.

[0052] Comparative Example 5 is a drilling fluid that differs from Example 4 in that the polymer thickener is replaced with another thickener, high-viscosity cellulose, in an amount of 2 parts. The other raw material composition and preparation method are the same.

[0053] IV. Drilling Fluid Performance Testing The drilling fluids of Comparative Examples 3 and 4, and Examples 4 to 6 were stirred at high speed for 20 minutes, and their rheological properties were measured using a six-speed rotational viscometer. The filtration loss was then measured, and the test results are shown in Table 4.

[0054] Table 4 Test Results .

[0055] As shown in Table 4, from Examples 4 to 6, the apparent viscosity of the drilling fluid system gradually increased and the filtration loss decreased with the increase of the polymer thickener dosage. Since the apparent viscosity and dynamic shear force of Examples 4 and 5 were not significantly different and the filtration loss was still above 5 mL, it indicates that Example 6 better meets the requirements for rheological control and low filtration loss under high salinity conditions. Comparative Example 3, which did not add any treatment agent, and Comparative Example 4, which only did not add polymer thickener, had very low apparent viscosity and high filtration loss, indicating that the addition of polymer thickener plays a key role in the rheological control and filtration loss reduction of the drilling fluid system. Compared to Comparative Example 5, which added another thickener, although the apparent viscosity increased, the filtration loss reduction effect was not significant, and the thickening effect of Examples 4 to 6 was significantly better.

[0056] V. Salt resistance test Due to the experimental design, Example 6 itself contains 10% NaCl. When conducting the salt resistance test, it is only necessary to modify and replace the NaCl content. That is, quantitatively weigh different mass fractions of NaCl and add them to the anti-brine drilling fluid system described in Example 6. After thorough stirring, the rheological properties and filtration loss of the drilling fluid are measured. The results are shown in Table 5.

[0057] Table 5. Rheological properties and filtration loss tests of NaCl with different mass fractions added to the anti-brine drilling fluid system in Example 6. .

[0058] Analyzing the data in Table 5, different proportions of salt were added to the anti-brine drilling fluid in ascending order, and the drilling fluid performance was tested. When the salt content reached saturation of 33%, the rheological properties and filtration loss of the drilling fluid remained within a controllable range, indicating that the system has good resistance to salt contamination.

[0059] VI. Anti-calcium performance test Due to the experimental design, Example 6 itself contains 10% NaCl. In order to test the anti-calcium performance, the anti-brine drilling fluid used is different from that in Example 6 in that NaCl is not added. The composition and preparation method of other raw materials are the same. On this basis, CaCl2 of different mass fractions is quantitatively weighed and added to the anti-brine drilling fluid system. After thorough stirring, the rheological properties and filtration loss of the drilling fluid are measured. The results are shown in Table 6.

[0060] Table 6. Rheological properties and filtration loss tests of CaCl2 with different mass fractions added to the brine-resistant drilling fluid system of Example 6. .

[0061] Analyzing the data in Table 6, different proportions of calcium were added to the anti-brine drilling fluid in ascending order, and the drilling fluid performance was tested. When the calcium content reached 15%, the drilling fluid rheology and filtration loss still maintained good rheology and low filtration loss, indicating that the system has good resistance to calcium contamination.

[0062] Six: The mud cake effect and mud cake SEM image of the brine-resistant drilling fluid prepared by this invention in fresh water-based slurry and 15% calcium-based slurry are shown below. Figure 2 As shown.

[0063] In summary, the brine-resistant drilling fluid of the present invention exhibits excellent rheological properties, filtration loss reduction properties, and inhibition properties in high-salt and high-calcium environments, and the synergistic effect of each additive is significant, which can meet the drilling requirements of high-mineralization formations.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A polymeric tackifier having the following structural formula: ; in, The ranges of x, y, and z are (60-70), (15-20), and (15-20), respectively. The polymer tackifier is characterized by being prepared by a method comprising the following steps: S1. Add 250 parts by weight of deionized water to a beaker, and while stirring, add 8 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid. Stir for 10 minutes, adjust the pH of the system to 7-8, and stir evenly to obtain mixture 1. S2. Under stirring conditions, add 8 parts by weight of acrylamide and 5 parts by weight of sulfonic acid to mixture 1, and then add 0.02~0.1 parts by weight of N,N'-methylenebisacrylamide. Stir for 10~20 minutes to obtain mixture 2. S3. Transfer the mixture 2 to the reactor. Under stirring conditions, remove oxygen by purging with nitrogen for 30 minutes, then raise the temperature and maintain it at 60±3℃. Dissolve 0.1~0.3 parts by weight of ammonium persulfate in 5 parts by weight of water and add it to the reactor. Continue stirring to carry out the polymerization reaction for 4~5 hours to obtain the mixture 3. S4. After the reaction is complete, stop heating and cool. Then, repeatedly soak and wash the product with detergent 3-5 times to obtain mixture 4. S5. Place the mixture 4 in an oven for 24-30 hours at a temperature of 45-60℃. After drying, take it out and crush it to obtain the polymer thickener product powder. The sulfonic acid is selected from one or more of sodium methacrylate sulfonate, sodium vinyl sulfonate, and sodium allyl sulfonate.

2. The use of the polymer tackifier according to claim 1, characterized in that, This polymer thickener is used to prepare a brine-resistant drilling fluid; wherein the brine-resistant drilling fluid is resistant to 33% NaCl and 15% CaCl2.

3. A drilling fluid resistant to brine intrusion, characterized in that, The raw materials include the following parts by weight: 40 parts bentonite, 2 parts sodium hydroxide, 10-20 parts of the polymer thickener as described in claim 1, 15 parts modified starch, 15 parts hydrolyzed polyacrylonitrile ammonium salt, and 1000 parts water.

4. The method for preparing the brine-resistant drilling fluid according to claim 3, characterized in that, Includes the following steps: S1. First, mix 1000 parts water with 40 parts bentonite, stir thoroughly for 20 minutes at 10000 r / min, and then cure at room temperature for 24 hours to form mixture 1. S2. Under stirring conditions of 8000~10000r / min, slowly and evenly add 10~20 parts of polymer thickener to mixture 1, stir for 15min until uniform, then add 15 parts of modified starch and 15 parts of hydrolyzed polyacrylonitrile ammonium salt in sequence, stir for 20min to form mixture 2. S3. Add NaOH to adjust the pH value of mixture 2, and stir thoroughly for 10 minutes at 1000 r / min to obtain the brine-resistant drilling fluid.

Citation Information

Patent Citations

  • High-salinity water-based drilling fluid and preparation method thereof

    CN112048289A

  • High-calcium-resistance ultrahigh-density drilling fluid system as well as preparation method and application thereof

    CN115991978A

  • Temperature-resistant and salt-resistant copolymer with filtration loss reducing, viscosity increasing and lubricating properties as well as preparation method and application of temperature-resistant and salt-resistant copolymer

    CN119192478A