Neodymium-iron-boron magnet and preparation method thereof
By applying an alternating oscillating attenuating magnetic field perpendicular to the static magnetic field in neodymium iron boron magnetic powder, the problem of carbon residue in neodymium iron boron magnets was solved, the orientation degree and magnetic properties were improved, and efficient mass production was achieved.
Patent Information
- Application Number
- CN202410961929.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2026-01-20
AI Technical Summary
In the preparation of NdFeB magnets, existing technologies involve adding lubricants to improve the flowability of magnetic powder, which leads to carbon residue and reduces the volume percentage of the main phase grains, affecting the remanence and energy product of the magnet. At the same time, the process is complex and not conducive to mass production and improving orientation.
By applying an alternating oscillating attenuated magnetic field perpendicularly to a static magnetic field, the agglomeration of NdFeB magnetic powder is first broken up, and then oriented and pressed in a predetermined oriented static magnetic field. Combined with sintering and heat treatment, a high-orientation NdFeB magnet is prepared.
The orientation degree and magnetic properties of NdFeB magnets have been improved, with an orientation degree exceeding 98%, a remanence of 14–16 kGs, and a magnetic energy product of 48–58 MGOe. The process has been simplified, making it suitable for mass production.
Smart Images

Figure CN121366788A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application belongs to the field of Nd-Fe-B magnets, in particular, relates to a Nd-Fe-B magnet and a preparation method thereof. BACKGROUND
[0002] Sintered Nd-Fe-B magnets have been widely used in aerospace, wind power, high-speed rail, new energy vehicles and various consumer electronics due to their excellent magnetic properties. With the continuous development of application fields, it is required that the magnets have higher magnetic properties. Magnetic field orientation is one of the key technologies for manufacturing high-performance sintered permanent magnets, and improving the orientation degree of Nd-Fe-B magnetic powder in the compaction process has an important influence on the magnetic properties of the magnet.
[0003] In order to improve the orientation degree, a certain amount of lubricant is usually added to the magnetic powder to improve the flowability of the magnetic powder. Since the lubricant cannot be completely volatilized during the sintering process, the residual carbon element in the magnet is easy to combine with rare earth elements to form a rare earth-rich phase at the grain boundary, which reduces the volume percentage of the main phase grain and is not conducive to improving the remanence and magnetic energy product of the magnet.
[0004] To solve the above problems, one prior art discloses a Nd-Fe-B powder compaction machine, which solves the problem of difficulty in rotating the magnetic powder during compaction orientation by first filling the magnetic powder into a rubber mold, then applying an intermittent positive and negative orientation pulse magnetic field on the magnetic powder, and the orientation magnetic field is perpendicular to the pressing direction. After pressing, a reverse magnetic field is applied to demagnetize, solving the problem of difficulty in rotating the magnetic powder during compaction orientation. Another prior art discloses a preparation method of high-performance magnets, which fills the magnetic powder into a rubber mold, then repeatedly applies a pulse magnetic field with a field strength greater than 10 kOe for repeated magnetization, then cold isostatic pressing in a static magnetic field to obtain high-performance magnets. However, the two technical solutions described above are not conducive to mass production due to the complexity of the process, and the effect of improving the orientation degree of the magnet is not good.
[0005] The contents of the background art section merely represent the best of the inventor's knowledge and do not necessarily represent the prior art in the field. SUMMARY
[0006] The purpose of the present application is to provide a Nd-Fe-B magnet and a preparation method thereof.
[0007] The method for preparing a Nd-Fe-B magnet provided by the present application comprises:
[0008] obtaining a Nd-Fe-B magnetic powder;
[0009] putting the Nd-Fe-B magnetic powder into a mold, and making the Nd-Fe-B magnetic powder in a loose state in the mold;
[0010] applying an alternating oscillation decay magnetic field to the Nd-Fe-B magnetic powder in the mold;
[0011] orienting and pressing in a predetermined orientation static magnetic field, wherein the magnetic field direction of the predetermined orientation static magnetic field is perpendicular to the magnetic field direction of the alternating oscillation decay magnetic field; and
[0012] post-processing the compact to obtain the Nd-Fe-B magnet.
[0013] In some embodiments of the present application, the initial magnetic field strength of the applied alternating oscillation decay magnetic field is 3.0-8.0T, and the applied alternating oscillation decay magnetic field is at least two periods.
[0014] In some embodiments of the present application, the loose bulk density of the Nd-Fe-B magnetic powder is 1.4-1.6g / cm 3 .
[0015] In some embodiments of the present application, before the Nd-Fe-B magnetic powder is put into the mold, the method further comprises:
[0016] adding an additive to the Nd-Fe-B magnetic powder and mixing uniformly.
[0017] In some embodiments of the present application, the amount of the additive added is less than or equal to 0.1wt% of the weight of the Nd-Fe-B magnetic powder.
[0018] In some embodiments of the present application, the strength of the predetermined orientation static magnetic field is 0.5-1.5T.
[0019] In some embodiments of the present application, the composition of the Nd-Fe-B magnetic powder is R x B y Co z M a Fe bal , wherein R is one or more rare earth elements with Nd as a necessary element, M is one or more of Cu, Ga, Al, Ti, Zr, Nb, Sn, and Ni; x=28.0-29.5, y=0.96-1.0, z=0.1-2.0, a=0-1.0, and bal is the balance in terms of mass percentage.
[0020] In some embodiments of the present application, the median particle size D50 of the Nd-Fe-B magnetic powder is 1.5-4μm.
[0021] In some embodiments of the present application, the post-processing comprises sintering and heat treatment; the sintering temperature is 1020-1080℃, and the time is 1-3h; the heat treatment comprises primary heat treatment and secondary heat treatment, the primary heat treatment temperature is 800-950℃, and the time is 1-3h, and the secondary heat treatment temperature is 450-650℃, and the time is 1-6h.
[0022] The neodymium-iron-boron magnet with high orientation degree provided by the application is prepared by the method.
[0023] In some embodiments of the application, the orientation degree of the neodymium-iron-boron magnet is greater than 98%, the residual magnetism is 14-16 kGs, and the magnetic energy product is 48-58 MGOe.
[0024] The application adopts an alternating oscillation decay magnetic field, and the direction of the magnetic field is perpendicular to the direction of the static magnetic field, so that the agglomeration of the magnetic powder can be dispersed, and the influence of the non-parallel magnetic force lines on the orientation of the magnetic powder can be reduced.
[0025] Additional aspects and advantages of the application will be set forth in part in the description which follows, and in part will become apparent to those skilled in the art upon examination of the following description and the accompanying drawings or can be learned by practice of the application. BRIEF DESCRIPTION OF DRAWINGS
[0026] The accompanying drawings, which form a part of the disclosure, are included to provide further understanding of the disclosure and are incorporated in and constitute a part of the disclosure. The illustrative embodiments of the disclosure and their specification are for purposes of explanation and do not properly limit the disclosure.
[0027] Figure 1 The preparation process flow chart of the neodymium-iron-boron magnet provided by an embodiment of the application. DETAILED DESCRIPTION
[0028] In the following, only certain example embodiments are simply described. As those skilled in the art can recognize, the described embodiments can be modified in various different ways without departing from the spirit or scope of the application. Therefore, the drawings and the description are considered to be exemplary in nature rather than limiting.
[0029] Considering the measurements discussed and the errors associated with the measurement of a particular quantity (i.e., the limitations of the measurement system), as used herein, "about" or "approximately" includes the stated value and means within an acceptable range of deviation from the particular value as determined by one of ordinary skill in the art. For example, "about" can mean within one or more standard deviations, or within ± 30%, ± 20%, ± 10%, or ± 5% of the stated value.
[0030] The inventors of the application found that, due to the small particle size of the neodymium-iron-boron magnetic powder (also referred to as "magnetic powder" in the following part of the description), under certain conditions, for example, when the surface of the pole head of an electromagnet generating a static magnetic field has a weak magnetic field, the magnetic powder particles are prone to spontaneous magnetization, and the agglomeration between the magnetized particles is prone to occur due to the static magnetism, and the powder particles are also prone to agglomerate more closely due to van der Waals force, which is not conducive to the improvement of the orientation degree of the magnetic powder particles under the action of the orientation static magnetic field.
[0031] Further, the inventors have also found that if a pulse magnetic field with a large field strength is applied in order to break up the agglomeration between the magnetic powders, the magnetic lines of force in the solenoid generating the pulse magnetic field are difficult to be parallel, which will affect the orientation consistency between the magnetic powders in a loose state after the pulse magnetic field is applied, and is not conducive to the improvement of the orientation degree of the compact after pressing.
[0032] Based on the above research, the present application provides a method for preparing a neodymium-iron-boron magnet, as shown in the following steps S1-S5. Figure 1
[0033] S1: obtaining a neodymium-iron-boron magnetic powder.
[0034] Optionally, the composition of the neodymium-iron-boron magnetic powder is R x B y Co z M a Fe bal , wherein R is one or more than one rare earth element with Nd as a necessary element; M is one or more of Cu, Ga, Al, Ti, Zr, Nb, Sn, and Ni; x = 28.0-29.5, y = 0.96-1.0, z = 0.1-2.0, a = 0-1.0, and bal is the balance in terms of mass percentage. Optionally, R also includes La, Pr, Ce, Dy, Tb, etc. The content of the rare earth element cannot be too much, too much of which will cause the remanence of the magnet to decrease, which is not conducive to obtaining a high-performance magnet with high remanence. In some specific embodiments, the content of the rare earth element can be 28.0wt%, 28.1wt%, 28.2wt%, 28.3wt%, 28.4wt%, 28.5wt%, 28.6wt%, 28.7wt%, 28.8wt%, 28.9wt%, 29.0wt%, 29.1wt%, 29.2wt%, 29.3wt%, 29.4wt%, or 29.5wt%.
[0035] Optionally, the median particle size D50 of the neodymium-iron-boron magnetic powder is 1.5-4μm. Further optionally, the median particle size D50 of the neodymium-iron-boron magnetic powder is 2.5-3.5μm. A too large particle size of the magnetic powder will affect the performance of the magnet. In some specific embodiments, the median particle size D50 of the neodymium-iron-boron magnetic powder can be 2.5μm, 2.6μm, 2.7μm, 2.8μm, 2.9μm, 3μm, 3.1μm, 3.2μm, 3.3μm, 3.4μm, or 3.5μm.
[0036] Optionally, the loose density of the neodymium-iron-boron magnetic powder is 1.4-1.6g / cm 3 . If the loose density is higher, it will be not conducive to breaking up the agglomeration of the magnetic powders by the alternating oscillation decay magnetic field, and further not conducive to the particle turning of the magnetic powders in the static magnetic field with a low pressing type. In some specific embodiments, the loose density of the neodymium-iron-boron magnetic powder can be 1.4g / cm3 1.42 g / cm 3 1.44 g / cm 3 1.46 g / cm 3 1.48 g / cm 3 1.5 g / cm 3 1.52 g / cm 3 1.54 g / cm 3 1.56 g / cm 3 1.57 g / cm 3 1.58 g / cm 3 .
[0037] When the magnetic powder is self-made, optionally, the preparation step comprises:
[0038] preparing an alloy rapid solidification sheet;
[0039] hydrogen crushing the alloy rapid solidification sheet to obtain a coarse powder; and
[0040] airflow milling the coarse powder to obtain a fine powder.
[0041] The alloy raw materials can be prepared according to the composition, then melted in a vacuum melting furnace, and the alloy is cast by using a rapid solidification casting sheet technology to obtain a rapid solidification alloy sheet with an average thickness of 0.2-0.4 mm. Then hydrogen crushing is performed to obtain a coarse powder, and then airflow milling is performed on the coarse powder to obtain a fine powder with a median particle size D50 of 1.5-4 μm.
[0042] S2: Placing the Nd-Fe-B magnetic powder into a mold and allowing the Nd-Fe-B magnetic powder to be in a loose state in the mold.
[0043] Here, the mold can be a mold of any shape, which is selected according to the shape of the magnet required.
[0044] In other embodiments of the present application, before placing the Nd-Fe-B magnetic powder into the mold, the method of the present application can further comprise: adding an additive to the Nd-Fe-B magnetic powder and mixing uniformly. The additive can be an antioxidant, a lubricant, etc.
[0045] Optionally, the amount of the additive added is less than or equal to 0.1 wt% of the weight of the Nd-Fe-B magnetic powder. If the amount of the additive is too much, the carbon content of the magnet prepared will also be high, which is not conducive to the improvement of the remanence of the magnet. In some specific embodiments, the amount of the additive added can be 0.1 wt%, 0.08 wt%, 0.06 wt%, 0.04 wt%, 0.02 wt% or 0.01 wt% of the weight of the Nd-Fe-B magnetic powder.
[0046] S3: Applying an alternating oscillation decay magnetic field to the Nd-Fe-B magnetic powder in the mold.
[0047] Optionally, the initial magnetic field strength of the applied alternating oscillation decay magnetic field is 3.0-8.0T. In the present application, the purpose of applying the alternating oscillation decay magnetic field is to disperse the magnetic powder agglomerates, and a magnetic field that is too small cannot achieve the dispersion function, and a magnetic field that is too large can magnetize the magnetic powder. In some specific embodiments, the size of the applied alternating oscillation decay magnetic field can be 3T, 3.3T, 3.6T, 3.9T, 4.2T, 4.5T, 4.8T, 5.1T, 5.4T, 5.7T, 6.2T, 6.7T, 7.1T, 7.7T or 8T.
[0048] Optionally, the applied alternating oscillation decay magnetic field is at least two periods. With the change of the current direction, the magnetic field direction will cycle once in a positive and negative direction in one period. The application of a magnetic field of at least two periods can effectively disperse the magnetic powder agglomerates. Further optionally, the alternating oscillation decay magnetic field is applied for two to six periods.
[0049] In the present application, the magnetic field direction of the applied alternating oscillation decay magnetic field is perpendicular to the magnetic field direction of the predetermined orientation static magnetic field in the subsequent orientation.
[0050] In the present application, the alternating oscillation decay magnetic field is applied, and the magnetic field direction is perpendicular to the static magnetic field direction, which not only disperses the magnetic powder agglomerates, but also reduces the influence of the magnetic field magnetic force line that is not parallel to the orientation of the magnetic powder. The main reason is that although the alternating oscillation coil produces a relatively large magnetic field strength, the internal magnetic force line cannot be completely parallel, but after the alternating oscillation decay magnetic field is applied to the loose magnetic powder, due to the large demagnetizing field of the magnetic powder itself, the residual magnetism of the magnetic powder caused by the alternating oscillation decay magnetic field is very weak. In addition, the alternating oscillation coil and the subsequent direct current steady field (the predetermined orientation static magnetic field in the subsequent orientation) are perpendicular, so that the magnetic powder after experiencing the alternating oscillation decay magnetic field can be basically regarded as the dispersed and non-oriented state without agglomeration, and the orientation direction of the magnetic powder relies entirely on the subsequent predetermined orientation static magnetic field in the orientation.
[0051] S4: orientation and molding in the predetermined orientation static magnetic field to obtain a compact.
[0052] As described above, the magnetic field direction of the predetermined orientation static magnetic field is perpendicular to the magnetic field direction of the alternating oscillation decay magnetic field. Optionally, the strength of the predetermined orientation static magnetic field is 0.5-1.5T. If the static magnetic field is too strong, the magnetic force lines between the poles of the electromagnet generating the static magnetic field will be more curved and divergent, which is not conducive to improving the orientation degree of the compact, and may result in a decrease in the orientation consistency of the whole magnet. In addition, a larger static magnetic field may increase the friction between the pole and the magnetic powder, affecting the orientation of the magnet. In some specific embodiments, the strength of the predetermined orientation static magnetic field can be 0.5T, 0.6T, 0.7T, 0.8T, 0.9T, 1T, 1.1T, 1.2T, 1.3T, 1.4T or 1.5T.
[0053] S5: performing post-processing on the compact to obtain a neodymium-iron-boron magnet.
[0054] Optionally, the post-processing includes sintering and heat treatment. The sintering temperature can be 1020-1080℃, and the time can be 1-3h. In some specific embodiments, the sintering temperature can be 1020℃, 1030℃, 1040℃, 1050℃, 1060℃, 1070℃ or 1080℃, and the time can be 1h, 1.5h, 2h, 2.5h or 3h.
[0055] Optionally, the heat treatment includes two-stage heat treatment (i.e., primary heat treatment and secondary heat treatment), which is conducive to improving the performance of the magnet. Optionally, the temperature of the primary heat treatment is 800-950℃, and the time is 1-3h. In some specific embodiments, the temperature of the primary heat treatment can be 800℃, 820℃, 840℃, 860℃, 880℃, 900℃, 920℃, 940℃ or 950℃, and the time can be 1h, 1.5h, 2h, 2.5h or 3h. Optionally, the temperature of the secondary heat treatment is 450-650℃, and the time is 1-6h. In some specific embodiments, the temperature of the secondary heat treatment can be 450℃, 470℃, 490℃, 510℃, 530℃, 550℃, 570℃, 590℃, 610℃, 630℃ or 650℃, and the time can be 1h, 2h, 3h, 4h, 5h or 6h.
[0056] The above method provided by the present application can obtain a neodymium-iron-boron magnet with high orientation degree and good performance.
[0057] The present application further provides a neodymium-iron-boron magnet prepared by the above method.
[0058] Optionally, the orientation degree of the neodymium-iron-boron magnet is >98%. For example, it can be 98.1%, 98.2%, 98.3%, 98.4%, 98.5%, 98.6%, 98.7% or 98.8%. Compared with the magnet provided by the prior art, the orientation degree is increased by about 1%.
[0059] Optionally, the remanence of the Nd-Fe-B magnet provided by the present application is 14-16 kGs, and the magnetic energy product is 48-58 MGOe. In some specific embodiments, the remanence of the Nd-Fe-B magnet can be 14 kGs, 14.4 kGs, 14.8 kGs, 15.2 kGs, 15.6 kGs or 16 kGs. In some specific embodiments, the magnetic energy product of the Nd-Fe-B magnet can be 48 MGOe, 50 MGOe, 52 MGOe, 54 MGOe, 56 MGOe or 58 MGOe.
[0060] The present application will be described below with reference to specific embodiments. The values of the process conditions taken in the following examples and comparative examples are exemplary, and the values of the ranges thereof are as shown in the foregoing summary of the application. For the process parameters not specifically mentioned, conventional techniques can be used. Unless specifically indicated, the reagents and instruments used in the technical solutions provided by the present application can be purchased from conventional channels or the market. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict. The test methods used in the following examples and comparative examples are conventional experimental methods in the art, unless otherwise specified.
[0061] Example 1
[0062] In this embodiment, a Nd-Fe-B magnet is prepared, and the specific steps are as follows:
[0063] 1) The raw materials are prepared according to the mass percentage ratio of (PrNd) 29.5 B 0.98 Co 1.0 Cu 0.12 Ga 0.1 Zr 0.15 Fe bal The raw materials are prepared. Melting is carried out in a vacuum melting furnace, and the vacuum degree is 10 -3 Pa, and the alloy is cast by using the rapid solidification casting technology, the cooling roll rotation speed is controlled to be 1 m / s, and the average thickness of the rapidly solidified alloy sheet is 0.3 mm.
[0064] 2) The obtained rapidly solidified alloy sheet is placed in a rotary hydrogen breaking furnace, and after the furnace chamber is cleaned by multiple vacuum-pumping-argon-filling-vacuum-pumping circulation operations, hydrogen is filled to perform hydrogen absorption breaking, the hydrogen absorption time is 1 h, and the pressure is maintained for about 2 hours to allow the rapidly solidified alloy sheet to be fully hydrogen absorbed and broken. Then, vacuum dehydrogenation is carried out by heating to about 550℃, and finally the coarse powder with a particle size of about 1 mm is obtained.
[0065] 3) The obtained coarse powder is mixed uniformly after adding an antioxidant by using a three-dimensional mixer, and then placed in a nitrogen jet mill for further breaking. During the breaking process, the pressure in the grinding chamber is stabilized at about 0.7 MPa, and the D50 of the finally obtained powder is about 3.5 μm, and the loose bulk density is about 1.5 g / cm 3 .
[0066] 4) Add 0.05wt% of the neodymium-iron-boron magnetic powder based on the weight of the neodymium-iron-boron magnetic powder to obtain a mixed powder.
[0067] 5) Fill the mixed powder into a square mold uniformly, the powder loading is 300g, the cross-sectional size of the mold cavity is 60x50mm, and 50mm is the orientation direction.
[0068] 6) Turn on the alternating oscillation coil magnetic field device, set the initial magnetic field strength to 3.5T and the frequency to 50Hz, oscillate the magnetic powder in the positive and negative magnetic field, and the oscillation time is 10s (two periods). The magnetic field direction of the alternating oscillation decay magnetic field is perpendicular to the magnetic field direction of the predetermined orientation static magnetic field.
[0069] 7) Turn off the pulse coil magnetic field device, move the magnetic powder to the predetermined orientation static magnetic field position, set the static magnetic field strength to 1.5T and the action time to 30s, perform the orientation compression step, and make the magnetic powder in the mold orient along the predetermined direction to obtain a well-oriented green magnet body, and the compression density is about 4.3g / cm 3 .
[0070] 8) Sinter and heat treat the compression body, the sintering temperature is 1050℃ and the holding time is 2h, the first-stage heat treatment temperature is 920℃ and the holding time is 2h; the second-stage heat treatment temperature is 480℃ and the holding time is 2h; and the final neodymium-iron-boron magnet is obtained.
[0071] Measure the magnetic properties, carbon content and orientation degree of the obtained neodymium-iron-boron magnet at each position, as shown in Tables 1 and 2.
[0072] Among them, for orientation degree measurement, three positions of upper, middle and lower on the edge and corner of the magnet and three positions of upper, middle and lower in the center are selected to process samples, and the sample specification is 10x10x10mm, and the orientation degree is measured. The specific method is as follows:
[0073] Test the magnet sample to process a cube, and the directions of the normal lines of each face of the cube are marked as a, b and c directions, wherein the c direction corresponds to the magnetic orientation direction of the magnet, and the a direction and the b direction are two mutually perpendicular directions perpendicular to the magnetic orientation direction of the magnet. After the a, b and c directions are saturated and magnetized by a saturation magnetizing field, the magnetic dipole moments are measured and recorded as jx, jy and jz. The orientation degree of the sample is calculated by the formula f=jz / (jx 2 +jy 2 +jz 2 ) 1 / 2 .
[0074] Comparative Example 1
[0075] This comparative example prepares a neodymium-iron-boron magnet, which is different from Example 1 only in that there is no step 6), and the mold filled with magnetic powder is directly placed in the predetermined orientation static magnetic field for orientation compression.
[0076] The orientation degree and magnetic properties of the obtained Nd-Fe-B magnets were measured, and are shown in Tables 1 and 2.
[0077] Example 2
[0078] This example prepared a Nd-Fe-B magnet, which was different from Example 1 in that the mass percentage ratio in step 1) was (PrNd) 28.5 B 0.98 Co 1.0 Cu 0.12 Ga 0.1 Zr 0.15 Fe bal The raw materials were prepared.
[0079] The magnetic properties, carbon content and orientation degree of samples from different parts of the obtained Nd-Fe-B magnets were measured, and are shown in Tables 2 and 3.
[0080] Comparative Example 2
[0081] This comparative example prepared a Nd-Fe-B magnet, which was different from Example 2 only in that there was no step 6), and the mold containing the magnetic powder was directly placed in a predetermined orientation static magnetic field to perform orientation compaction.
[0082] The magnetic properties, carbon content and orientation degree of samples from different parts of the obtained Nd-Fe-B magnets were measured, and are shown in Tables 2 and 3.
[0083] Example 3
[0084] This example prepared a Nd-Fe-B magnet, which was different from Example 1 in that the mass percentage ratio in step 1) was (PrNd) 29 B 0.98 Co 1.0 Cu 0.12 Ga 0.1 Zr 0.15 Fe bal The raw materials were prepared, the D50 of the powder obtained in step 3) was about 2.8 μm, and the initial magnetic field strength of the alternating oscillation decay magnetic field in step 6) was 3.0 T, and the oscillation time was 15 s (three periods).
[0085] The magnetic properties and carbon content of the obtained Nd-Fe-B magnets were measured, and are shown in Table 2.
[0086] Comparative Example 3
[0087] This comparative example prepared a Nd-Fe-B magnet, which was different from Example 3 only in that there was no step 6), and the mold containing the magnetic powder was directly placed in a predetermined orientation static magnetic field to perform orientation compaction.
[0088] The magnetic properties and carbon content of the obtained Nd-Fe-B magnets were measured, and are shown in Table 2.
[0089] Example 4
[0090] This example prepared a Nd-Fe-B magnet, which was different from Example 1 in that the D50 of the powder obtained in step 3) was about 3.1 μm, and the initial magnetic field strength of the AC oscillation decay magnetic field in step 6) was 4.0 T.
[0091] The magnetic properties of the obtained Nd-Fe-B magnet were measured, and are shown in Table 2.
[0092] Comparative Example 4
[0093] This comparative example prepared a Nd-Fe-B magnet, which was different from Example 4 only in that there was no step 6), and the mold containing the magnetic powder was directly placed in a predetermined orientation static magnetic field to perform orientation compaction.
[0094] The magnetic properties of the obtained Nd-Fe-B magnet were measured, and are shown in Table 2.
[0095] Example 5
[0096] This example prepared a Nd-Fe-B magnet, which was different from Example 1 in that the magnetic field strength of the static magnetic field in step 7) was 2.0 T.
[0097] The magnetic properties, carbon content, and orientation degree of the samples of each part of the obtained Nd-Fe-B magnet were measured, and are shown in Table 2 and Table 4.
[0098] Table 1
[0099] Sample at magnet position Example 1 Comparative Example 1 Upper corner 98.2% 97.1% Mid corner 98.5% 97.4% Lower corner 98.3% 97.2% Upper middle 98.2% 97.2% Mid middle 98.8% 97.8% Lower middle 98.2% 97.3%
[0100] Table 2
[0101] Remanence / kGs Coercivity / kOe Max Energy Product / MGOe Carbon content / ppm Example 1 14.63 14.13 52.69 310 Comparative Example 1 14.52 14.06 51.43 295 Example 2 15.23 10.08 57.14 200 Comparative Example 2 15.11 10.01 56.13 220 Example 3 14.61 14.16 52.62 300 Comparative Example 3 14.48 14.08 51.16 290 Example 4 14.06 17.52 48.73 350 Comparative Example 4 13.85 17.56 46.81 330 Example 5 14.62 14.11 52.64 305
[0102] Table 3
[0103] Sample at magnet position Example 2 Comparative Example 2 Upper corner 98.6% 97.6% Mid corner 98.7% 97.7% Lower corner 98.5% 97.6% Upper middle 98.6% 97.7% Mid middle 98.8% 97.9% Lower middle 98.7% 97.8%
[0104] Table 4
[0105] Sample at magnet position Example 5 Upper corner 97.7% Mid corner 97.8% Lower corner 97.5% Upper middle 98.2% Mid middle 98.7% Lower middle 98.4%
[0106] From the above examples and comparative examples, it can be seen that the AC oscillation decay magnetic field is used to disperse the agglomerates of the magnetic powder, and the direction of the magnetic field is perpendicular to the direction of the static magnetic field, so that a Nd-Fe-B magnet with a high orientation degree can be obtained. In the case of a lower addition of antioxidant, the carbon content of the magnet is lower, and the orientation degree of the samples of each part of the magnet of Examples 1-4 is higher than that of Comparative Examples 1-4, and is greater than 98%, so that the overall orientation degree of the magnet is greater than 98%, and the remanence and the magnetic energy product are higher. In Example 5, the orientation degree of the corner sample is lower than that of the middle sample, and the orientation inside the magnet is not uniform.
[0107] Obviously, the above embodiments are only examples for clearly illustrating the present application, and are not intended to limit the implementation modes. Based on the above description, other different forms of changes or variations can also be made by those skilled in the art. Here, all the implementation modes do not need to be exhausted, and the obvious changes or variations derived therefrom are still within the protection scope of the present application.
Claims
1. A method of producing a neodymium-iron-boron magnet, characterized by, The method comprises: obtaining neodymium-iron-boron magnetic powder; putting the neodymium-iron-boron magnetic powder into a mold and allowing the neodymium-iron-boron magnetic powder to be in a loose state in the mold; applying an alternating oscillation decay magnetic field to the neodymium-iron-boron magnetic powder in the mold; performing orientation compression in a predetermined orientation static magnetic field to obtain a compact, wherein the magnetic field direction of the predetermined orientation static magnetic field is perpendicular to the magnetic field direction of the alternating oscillation decay magnetic field; and performing post-processing on the compact to obtain the neodymium-iron-boron magnet. The initial magnetic field strength of the applied alternating oscillation decay magnetic field is 3.0-8.0 T, and the alternating oscillation decay magnetic field is at least two periods.
2. The method of claim 1, wherein, Before putting the neodymium-iron-boron magnetic powder into the mold, the method further comprises:
3. The method of claim 1, wherein, The loose density of the Nd-Fe-B magnetic powder is 1.4-1.6 g / cm 3 .
4. The method of claim 1, wherein, adding an additive to the neodymium-iron-boron magnetic powder and mixing uniformly; wherein the additive is added in an amount less than or equal to 0.1 wt% of the weight of the neodymium-iron-boron magnetic powder. The strength of the predetermined orientation static magnetic field is 0.5-1.5 T.
5. The method of claim 1, wherein, The median particle size D50 of the neodymium-iron-boron magnetic powder is 1.5-4 μm.
6. The method of claim 1, wherein, The composition of the neodymium-iron-boron magnetic powder is R x B y Co z M a Fe bal , wherein R is one or more rare earth elements with Nd as a necessary element, M is one or more of Cu, Ga, Al, Ti, Zr, Nb, Sn, and Ni; x = 28.0-29.5, y = 0.96-1.0, z = 0.1-2.0, a = 0-1.0, and bal is the balance in terms of mass percentage.
7. The method of claim 1, wherein, The post-processing comprises sintering and heat treatment; the sintering temperature is 1020-1080 °C, and the time is 1-6 h; the heat treatment comprises primary heat treatment and secondary heat treatment, the primary heat treatment temperature is 800-950 °C, and the time is 1-3 h, the secondary heat treatment temperature is 450-650 °C, and the time is 1-6 h.
8. The method of claim 1, wherein, Prepared by the method of any one of claims 1-8.
9. A neodymium-iron-boron magnet, characterized by The orientation degree of the neodymium-iron-boron magnet is >98%, the remanence is 14-16 kGs, and the magnetic energy product is 48-58 MGOe.
10. The neodymium-iron-boron magnet according to claim 9, characterized in that