A battery separator, its preparation method and application
By introducing a gradient pore structure and oxygen- and nitrogen-containing functional groups into the lithium-ion battery separator, the problems of poor adhesion between the separator and the electrode and lithium dendrite growth in traditional lithium-ion battery are solved, achieving higher adhesion strength and uniform electrolyte distribution, thereby improving battery safety and cycle performance.
Patent Information
- Application Number
- CN202511343361.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-19
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-09-19
AI Technical Summary
Traditional lithium-ion batteries have poor adhesion between the separator and the electrode, high interfacial impedance, and lithium dendrite growth that can easily lead to safety hazards. Furthermore, uneven electrolyte wetting can cause localized polarization.
The battery separator adopts a layered structure, and the modification layer contains a gradient pore structure and oxygen- and nitrogen-containing functional groups. Functional groups are introduced through plasma or chemical grafting treatment to optimize the lithium-ion transport path.
It improves the adhesion strength between the separator and the electrode, inhibits lithium dendrite growth, reduces interfacial impedance, enhances the wetting performance and capacity retention of the electrolyte, and improves the safety performance of the battery.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of energy storage technology, and particularly relates to a battery separator, its preparation method and application. Background Technology
[0002] Traditional lithium-ion battery separators often use porous polyolefin membranes (such as polyethylene PE and polypropylene PP), but their strong surface inertness leads to poor adhesion to the electrodes and high interfacial impedance. In existing technologies, lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP), and lithium lanthanum zirconium oxide (LLZO) are commonly used as fast ion conductors to improve lithium-ion transport; however, their interfacial compatibility with polyolefin-based membranes is poor, and direct coating easily clogs pores, limiting electrolyte diffusion. Furthermore, uneven electrolyte wetting can easily cause localized polarization, exacerbating lithium dendrite growth, especially at battery corners where lithium plating is prone to occur, posing a safety hazard. Summary of the Invention
[0003] In order to overcome at least one of the problems existing in the prior art, one of the objectives of the present invention is to provide a battery separator that, through interface modification and gradient pore structure design, has high adhesion strength to the electrode, optimized lithium-ion transport path, and effectively suppresses lithium plating.
[0004] The second objective of this invention is to provide a method for preparing the above-mentioned battery separator.
[0005] The third objective of this invention is to provide a battery.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A first aspect of the present invention provides a battery separator, comprising a base film and a modification layer stacked thereon; the modification layer comprises a solid electrolyte and a binder; the modification layer is further modified with oxygen-containing functional groups and / or nitrogen-containing functional groups; the modification layer has a gradient pore structure, wherein the pore size gradually decreases from the interface between the modification layer and the base film toward the surface of the modification layer.
[0007] Preferably, the pore size of the interface between the modified layer and the base film is 100~300nm; for example, it can be any value of 100nm, 150nm, 200nm, 250nm or 300nm or any range between two.
[0008] Preferably, the pore size of the surface of the modified layer is 10~50nm; for example, it can be any value of 10nm, 20nm, 30nm, 40nm or 50nm or a range between any two.
[0009] Preferably, the pore size (D) at the interface between the modified layer and the base film is... max ) and the pore size (D) of the surface of the modified layer minThe ratio of (D) max / D min The value is 4 to 30; for example, it can be any value or a range between any two of 4, 5, 6, 7, 8, 10, 15, 20, 25 or 30; more preferably, it is 5 to 15.
[0010] Preferably, the pore size (D) at the interface between the modified layer and the base film is... max ) and the pore size (D) of the surface of the modified layer min The difference (D) max -D min The wavelength range is 70~290nm; for example, it can be any value or a range between any two of 70nm, 80nm, 100nm, 150nm, 180nm, 200nm, 220nm, 250nm, 280nm or 290nm; more preferably, it is 100~250nm.
[0011] The gradient pore structure of this invention can guide the uniform and orderly transport of lithium ions, effectively suppressing dendrite growth. The aforementioned limitation of the pore size ratio or pore size difference is beneficial for improving the ion transport gradient; if the ratio or difference is too small, the gradient effect is not obvious, and the optimization of the ion transport path is minimal; if the ratio or difference is too large, it may lead to a decrease in the mechanical strength of the dense surface layer or an increase in the difficulty of the fabrication process. Furthermore, the combined limitation of the aforementioned pore size ratio or pore size difference is beneficial for more effectively improving the ion transport gradient.
[0012] Preferably, the thickness of the modification layer is 1~5μm; for example, it can be any value of 1μm, 2μm, 3μm, 4μm or 5μm or a range between any two.
[0013] Preferably, the oxygen content in the modified layer is 5-15% by mass; for example, it can be any value of 5%, 8%, 10%, 12% or 15% or a range between any two.
[0014] Preferably, the nitrogen content in the modified layer is 1-5% by mass; for example, it can be any value of 1%, 2%, 3%, 4% or 5% or a range between any two.
[0015] By introducing oxygen- and nitrogen-containing functional groups, a stable structure can be formed with solvent molecules in the electrolyte, inhibiting electrolyte volatilization. Simultaneously, the ion transport pathway is optimized, promoting uniform electrolyte distribution and reducing localized evaporation. Furthermore, the synergistic effect between oxygen and nitrogen content and pore size gradient can further improve the membrane's capacity retention.
[0016] Preferably, the mass ratio (O / N) of oxygen to nitrogen in the modified layer is (0.75~15):1; for example, it can be any value or a range between any two of 0.75:1, 1:1, 2:1, 3:1, 5:1, 8:1, 10:1, 12:1 or 15:1; more preferably (1~10):1.
[0017] Controlling the appropriate oxygen-nitrogen mass ratio is beneficial for the synergistic effect of oxygen- and nitrogen-containing functional groups, which can form more stable and diverse hydrogen bonds or coordination bonds with various solvent molecules in the electrolyte (such as EC, DEC, etc.). This can more effectively suppress electrolyte volatilization and achieve better wetting performance, higher adhesion strength and better interfacial stability.
[0018] Preferably, the oxygen-containing functional group includes hydroxyl, carboxyl, or a combination thereof; more preferably, the oxygen-containing functional group includes hydroxyl and carboxyl.
[0019] Preferably, the nitrogen-containing functional group includes an amino group.
[0020] Preferably, the mass ratio of the solid electrolyte to the binder is (3~15):1; more preferably (4~12):1; and even more preferably (5~10):1.
[0021] Controlling the mass ratio of solid electrolyte to binder ensures the uniformity and mechanical strength of the modified layer.
[0022] Preferably, the solid electrolyte comprises at least one of lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP), or lithium lanthanum zirconium oxide (LLZO).
[0023] Preferably, the adhesive comprises at least one of polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyethylene oxide (PEO), sodium alginate, polytetrafluoroethylene (PTFE), polyvinylpyrrolidone (PVP), polyacrylonitrile (PAN), or polyvinyl alcohol (PVA); more preferably, the adhesive comprises at least one of polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), polyethylene oxide (PEO), or polytetrafluoroethylene (PTFE); even more preferably, the adhesive comprises polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), or a combination thereof.
[0024] In some embodiments of the present invention, the pore size of the base film is uniformly distributed.
[0025] Preferably, the pore size of the base film is 0.1~1μm; for example, it can be any value of 0.1μm, 0.3μm, 0.5μm, 0.8μm or 1μm or a range between any two.
[0026] Preferably, the base film is made of polyolefin; more preferably, the polyolefin includes polyethylene (PE), polypropylene (PP), or a combination thereof.
[0027] Preferably, the battery separator is a solid electrolyte battery separator.
[0028] A second aspect of the present invention provides a method for preparing a battery separator, comprising the following steps: dispersing a solid electrolyte and a binder in a solvent to form a slurry; introducing active functional groups into the slurry to form a modified slurry, wherein the active functional groups include oxygen-containing functional groups, nitrogen-containing functional groups, or combinations thereof; applying the modified slurry to the surface of a base film, drying, and roll forming to obtain the battery separator as described in the first aspect of the present invention.
[0029] Preferably, the active functional groups are introduced by means of plasma treatment, chemical grafting treatment, or a combination thereof.
[0030] Preferably, the plasma treatment specifically includes the following steps: subjecting the slurry to plasma treatment to form a modified slurry.
[0031] Preferably, the processing gas for plasma treatment includes oxygen, nitrogen, or a combination thereof; more preferably, the processing gas for plasma treatment includes oxygen and nitrogen; the volume ratio of oxygen to nitrogen can be 1:(0.5~2), for example 1:0.5, 1:1, 1:1.5, 1:2, etc.
[0032] Preferably, the plasma treatment power is 100~200W; for example, it can be any value of 100W, 120W, 150W, 180W or 200W or any range between two.
[0033] Preferably, the plasma treatment time is 1 to 10 minutes; for example, it can be any value of 1 minute, 3 minutes, 5 minutes, 7 minutes or 10 minutes or a range between any two.
[0034] Preferably, the treatment reagent for the chemical grafting treatment includes a coupling agent.
[0035] Preferably, the chemical grafting treatment specifically includes the following steps: mixing the slurry with a coupling agent and performing chemical grafting treatment to form a modified slurry.
[0036] Preferably, the coupling agent comprises an amino coupling agent; more preferably, the amino coupling agent comprises 3-aminopropyltrimethoxysilane (APTMS), 3-aminopropyltriethoxysilane (APTES), or a combination thereof; even more preferably, the amino coupling agent is selected from 3-aminopropyltriethoxysilane (APTES).
[0037] Preferably, the chemical grafting treatment temperature is 50~70℃; for example, it can be any value of 50℃, 55℃, 60℃, 65℃ or 70℃ or a range between any two.
[0038] Preferably, the chemical grafting treatment time is 1 to 3 hours; for example, it can be any value of 1 hour, 2 hours, or 3 hours, or a range between any two.
[0039] Preferably, the solvent includes an organic solvent, water, or a combination thereof; more preferably, the organic solvent includes at least one of N-methylpyrrolidone (NMP), acetone, toluene, isopropanol, or ethyl acetate.
[0040] Preferably, the modified slurry is applied to the surface of the base film by coating; more preferably, the coating speed is 0.1~1m / min; for example, it can be any value or a range between 0.1m / min, 0.3m / min, 0.5m / min, 0.7m / min or 1m / min.
[0041] Preferably, the drying temperature is 50~100℃; for example, it can be any value of 50℃, 60℃, 70℃, 80℃, 90℃ or 100℃ or a range between any two.
[0042] A third aspect of the present invention is to provide a battery comprising a battery separator as described in the first aspect of the present invention.
[0043] Preferably, the battery further includes an electrolyte; the solvent of the electrolyte includes at least one of ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), or propylene carbonate (PC); more preferably, the solvent of the electrolyte includes ethylene carbonate (EC), diethyl carbonate (DEC), or a combination thereof.
[0044] The battery separator provided by this invention can form a stable bond with solvent molecules (such as EC, DEC, etc.) in the electrolyte, thereby inhibiting electrolyte evaporation and achieving good wetting performance. The resulting battery has lower interfacial impedance and higher capacity retention.
[0045] Preferably, the battery is a solid-state electrolyte battery.
[0046] Preferably, the battery is a lithium-ion battery.
[0047] The gradient pore structure of the modification layer in the battery separator of this invention is beneficial to optimizing the lithium ion transport path, suppressing lithium plating, and resulting in a lithium-ion battery with good safety performance.
[0048] The beneficial effects of this invention are as follows: The invention introduces oxygen-containing and / or nitrogen-containing functional groups into the modification layer, which can form a stable structure with solvent molecules in the electrolyte, inhibiting electrolyte evaporation and achieving good wetting performance between the separator and the electrolyte. Furthermore, the gradient pore structure of the modification layer optimizes the ion transport path and facilitates capillary action, promoting uniform electrolyte distribution and reducing localized evaporation. Moreover, the gradient pore structure and functional groups work synergistically to optimize the electrolyte wetting path, significantly reducing the electrolyte evaporation rate, lowering interfacial impedance, reducing capacity decay due to electrolyte loss, and improving the adhesion strength between the separator and the electrode. The battery separator provided by this invention is beneficial for preparing batteries with good electrical performance, especially lithium-ion batteries. Detailed Implementation
[0049] The following specific embodiments further illustrate the content of the present invention in detail. It should also be understood that the following embodiments are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made by those skilled in the art based on the principles described herein are all within the scope of protection of the present invention. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make selections within a suitable range based on the description herein, and are not intended to be limited to the specific data in the examples below. Unless otherwise specified, the raw materials, reagents, or apparatus used in the following embodiments and comparative examples can be obtained from conventional commercial sources or by existing known methods.
[0050] In the following examples and comparative examples, the chemical formula of lithium aluminum titanium phosphate (LATP) is Li 1.3 Al 0.3 Ti 1.7 (PO4)3; The chemical formula of lithium aluminum germanium phosphate (LAGP) is Li 1.5 Al 0.5 Ge 1.5 (PO4)3.
[0051] Example 1 A battery separator is prepared by the following steps: 1) Slurry preparation: Take LATP powder (particle size 200nm) with a mass ratio of 8:1 and disperse it with polyvinylidene fluoride (PVDF) binder in NMP solvent, and stir for 1.5 hours to form a uniform slurry.
[0052] 2) Plasma treatment: The slurry is subjected to plasma treatment with a mixture of O2 / N2 gas (volume ratio 1:1), a treatment power of 150W, and a treatment time of 5 minutes, thereby introducing oxygen-containing (-OH, -COOH) functional groups to form a modified slurry.
[0053] 3) Coating and Roll Pressing: The modified slurry is coated onto the surface of a PE base film (pore size 200nm) at a coating speed of 0.5m / min and dried at 80℃; then, roll pressing is performed to form a modified layer; the modified layer has a thickness of 2μm and a gradient pore size structure, with the pore size gradually decreasing from the interface between the modified layer and the base film towards the surface of the modified layer. The pore size D at the interface between the modified layer and the base film is... max The pore size D on the surface of the modified layer is 200 nm. min The aperture ratio is 30 nm, and the pore size is D. max / D min The O / N mass ratio of the modified layer is 5:1, with a value of 6.67. A specific gradient pore structure is achieved by controlling the coating speed, drying temperature and time, roller pressure, and layer design.
[0054] Example 2 A battery separator is prepared by the following steps: 1) Slurry preparation: Take LATP powder (particle size 300nm) with a mass ratio of 6:1 and disperse it with polyacrylic acid (PAA) binder in deionized water, and stir for 1.5 hours to form a uniform slurry.
[0055] 2) Chemical grafting treatment: 3-aminopropyltriethoxysilane (APTES) is added to the slurry as a coupling agent for reaction at a temperature of 60°C for 2 hours, thereby introducing amino (-NH2) functional groups to form a modified slurry.
[0056] 3) Coating and Roll Pressing: The modified slurry was coated onto the surface of a PP base film (pore size 150nm) at a coating speed of 0.3m / min and dried at 70℃; then, roll pressing was performed to form a modified layer; the modified layer thickness was 3μm, and the modified layer had a gradient pore size structure, with the pore size gradually decreasing from the interface between the modified layer and the base film towards the surface of the modified layer. The pore size D at the interface between the modified layer and the base film was... max The pore size D on the surface of the modified layer is 150 nm. min The aperture ratio is 20 nm, and the pore size is D. max / D minThe O / N mass ratio of the modified layer is 0.75:1. A specific gradient pore structure is achieved by controlling the coating speed, drying temperature and time, roll pressure, and layer design.
[0057] Example 3 A battery separator is prepared by the following steps: 1) Slurry preparation: Take LATP powder (particle size 200nm) with a mass ratio of 10:1 and disperse it with polyethylene oxide (PEO) binder in NMP solvent, and stir for 1.5 hours to form a uniform slurry.
[0058] 2) Plasma treatment: The slurry is subjected to plasma treatment with O2 as the treatment gas, 200W as the treatment power, and 10 minutes as the treatment time, thereby introducing oxygen-containing (-OH, -COOH) functional groups to form a modified slurry.
[0059] 3) Coating and Roll Pressing: The modified slurry was coated onto the surface of a PP base film (pore size 200nm) at a coating speed of 0.3m / min and dried at 70℃; then, roll pressing was performed to form a modified layer; the modified layer thickness was 3μm, and the modified layer had a gradient pore size structure, with the pore size gradually decreasing from the interface between the modified layer and the base film towards the surface of the modified layer. The pore size D at the interface between the modified layer and the base film was... max The pore size D on the surface of the modified layer is 280 nm. min The aperture ratio is 20 nm, and the pore size is D. max / D min The O / N mass ratio of the modified layer is 15:1. A specific gradient pore structure is achieved by controlling the coating speed, drying temperature and time, roller pressure, and layer design.
[0060] Example 4 A battery separator, differing from Example 1, involves adjusting the slurry solid content and rolling process parameters to increase the pore size D at the interface between the modified layer and the base film. max The pore size D on the surface of the modified layer is 300 nm. min The aperture ratio is 10 nm, and the pore size is D. max / D min The value was 30; other raw materials and preparation conditions were the same as in Example 1.
[0061] Example 5 A battery separator, differing from Example 1, involves adjusting the slurry solid content and rolling process parameters to increase the pore size D at the interface between the modified layer and the base film. max The pore size D on the surface of the modified layer is 120 nm. min The aperture ratio is 30 nm, and the pore size is D. max / D min The value was 4; other raw materials and preparation conditions were the same as in Example 1.
[0062] Example 6 A battery separator, which differs from Example 1 in that LATP powder is replaced with an equal mass of LAGP powder; other raw materials and preparation conditions are the same as in Example 1.
[0063] Comparative Example 1 A battery separator (without functional group modification and with a gradient pore structure) differs from Example 1 in that step 2) is omitted in this example; in step 3), the slurry formed in step 1) is directly used for coating and roll forming, and the resulting modified layer has a gradient pore structure, which is the same as that in Example 1; other raw materials and preparation conditions are the same as those in Example 1.
[0064] Comparative Example 2 A battery separator (without functional group modification and without gradient pore structure) differs from Example 1 in that step 2) is omitted in this example; in step 3), the slurry formed in step 1) is directly used for coating and roll forming, and in step 3), the roll forming process is adjusted so that the modified layer has a uniformly distributed pore structure with a pore size of 50 nm; other raw materials and preparation conditions are the same as in Example 1.
[0065] Comparative Example 3 A battery separator (functionally modified, without gradient pore structure) is prepared by the following steps: 1) Slurry preparation: Take LATP powder (particle size 200nm) with a mass ratio of 8:1 and disperse it with polyvinylidene fluoride (PVDF) binder in NMP solvent, and stir for 1.5 hours to form a uniform slurry.
[0066] 2) Plasma treatment: The slurry is subjected to plasma treatment with a mixture of O2 / N2 gas (volume ratio 1:1), a treatment power of 150W, and a treatment time of 5 minutes, thereby introducing oxygen-containing (-OH, -COOH) functional groups to form a modified slurry.
[0067] 3) Coating and roll forming: The modified slurry is coated on the surface of the PE base film (pore size 200nm) at a coating speed of 0.5m / min and dried at 80℃; then roll forming is performed to form a modified layer; the thickness of the modified layer is 2μm. In this example, the modified layer is controlled to have a uniformly distributed pore structure through the roll forming process, and the pore size of the modified layer is 50nm.
[0068] The specific comparison of the schemes in Examples 1-5 and Comparative Examples 1-3 is shown in Table 1.
[0069] Table 1. Comparison of Examples 1-5 and Comparative Examples 1-3
[0070] Performance testing 1) Adhesion strength: Peel tests were performed on the diaphragms of the examples and comparative examples according to ASTM D903-98 (2025).
[0071] 2) Wetting time: The electrolyte was dropped onto the diaphragm surface of the examples and comparative examples, and the complete wetting time was recorded.
[0072] 3) Lithium plating inhibition rate: The separators of the examples and comparative examples were assembled into batteries. After the batteries had completed their working cycles, they were disassembled and the percentage of lithium plating area at the battery corners was observed by scanning electron microscopy (SEM).
[0073] 4) Cycle capacity retention: The separators of the examples and comparative examples were assembled into batteries, and the cycle capacity retention of the batteries was tested at 0.5C.
[0074] 5) Electrolyte retention rate: The separators of the examples and comparative examples were assembled into batteries. The fully charged batteries were stored at a high temperature of 60°C for 30 days. The electrolyte mass loss and electrolyte retention rate were calculated by weighing.
[0075] 6) Overall Performance Index P: A comprehensive indicator used to quantify the membrane's adhesion performance and ion transport efficiency, requiring P ≥ 8.0. The formula for calculating the Overall Performance Index P is as follows:
[0076] Where k1=0.8, k2=0.5; α and β are weighting coefficients, α=0.6, β=0.4; D max and D min [0%] and [N%] represent the maximum and minimum pore sizes of the separator modification layer, respectively; [O%] and [N%] represent the mass content of oxygen and nitrogen in the separator modification layer, respectively. The effective threshold is P≥8.0. When P≥8.0, the adhesion strength, wetting rate, and lithium plating inhibition ability of the separator reach a synergistic optimization state, meeting the requirements of high-performance batteries.
[0077] In Examples 1-6, [O%] is 5%-15%, and [N%] is 1%-5%.
[0078] The performance test results are shown in Table 2.
[0079] Table 2. Test results of membrane performance in Examples 1-6 and Comparative Examples 1-3
[0080] As shown in Table 2, the battery separators of Examples 1-6 of this invention, through functional group modification and gradient pore structure synergistic design, have a comprehensive performance index P that is significantly higher than that of the schemes in the comparative examples (P≥8.7 for Examples 1-6, P≤7.5 for Comparative Examples 1-3). The bonding strength is ≥14N / m, the wetting time is ≤130s, the corner lithium plating suppression rate is ≥92%, the capacity retention rate after 500 cycles is ≥91%, and the electrolyte retention rate is increased to over 90%. This effectively solves the problems of poor adhesion, high risk of lithium plating, cycle performance degradation, and electrolyte volatilization of existing lithium-ion battery separators.
[0081] In Comparative Example 1, no functional group modification was used, resulting in weak adhesion between the modified layer and the base film. The adhesion strength of the battery separator was only 6.5 N / m, indicating insufficient interfacial adhesion between the modified layer and the base film, which failed to meet the adhesion performance requirements of the battery separator. Furthermore, Comparative Example 1 failed to leverage the synergistic effect of specific oxygen and nitrogen content and pore size gradient, resulting in a low cycle capacity retention rate of only 78.4%. At the same time, the gradient pore structure was not combined with functional group modification, leading to a rapid electrolyte evaporation rate and a low electrolyte retention rate of only 72.3% after cycling. The wetting time was as long as 300 s, and the lithium plating inhibition rate was only 70%.
[0082] In Comparative Example 2, a uniform pore size structure was used instead of a gradient pore structure, which hindered electrolyte diffusion, extended the wetting time to 180s, and resulted in poor lithium plating inhibition, with a lithium plating inhibition rate of only 80%. The gradient pore structure was not combined with functional group modification, resulting in low cycle capacity retention (83.0%) and low electrolyte retention after cycling (78.0%).
[0083] Comparative Example 3 uses functional group modification but does not have a gradient pore structure, resulting in poor cycle capacity retention (89.0%) and electrolyte retention (76.8%), which is difficult to meet the requirements for battery separator use.
[0084] In summary, this invention introduces oxygen-containing and / or nitrogen-containing functional groups into the modification layer, which can form a stable structure with solvent molecules in the electrolyte, inhibiting electrolyte evaporation and achieving good wetting performance between the separator and the electrolyte. The gradient pore structure of the modification layer optimizes the ion transport path and facilitates capillary action, promoting uniform electrolyte distribution and reducing localized evaporation. Furthermore, the gradient pore structure and functional groups work synergistically to optimize the electrolyte wetting path, significantly reducing the electrolyte evaporation rate, lowering interfacial impedance, reducing capacity decay due to electrolyte loss, and improving the adhesion strength between the separator and the electrode. The battery separator of this invention is beneficial for preparing high-performance batteries, especially lithium-ion batteries.
Claims
1. A battery separator, characterized in that, The invention comprises a base film and a modification layer stacked together; the modification layer comprises a solid electrolyte and a binder; the modification layer is further modified with oxygen-containing functional groups and nitrogen-containing functional groups; the modification layer has a gradient pore structure in which the pore size gradually decreases from the interface between the modification layer and the base film toward the surface of the modification layer. The modified layer has an oxygen content of 5-15% by mass; the modified layer has a nitrogen content of 1-5% by mass; and the mass ratio of oxygen to nitrogen in the modified layer is (1-15):
1. The pore size at the interface between the modified layer and the base film is 100~300nm; the pore size on the surface of the modified layer is 10~50nm; and simultaneously satisfies the following: the ratio of the pore size at the interface between the modified layer and the base film to the pore size on the surface of the modified layer is 4~30; and the difference between the pore size at the interface between the modified layer and the base film and the pore size on the surface of the modified layer is 70~290nm.
2. The battery separator according to claim 1, characterized in that, The thickness of the modified layer is 1~5μm.
3. The battery separator according to claim 1, characterized in that, The oxygen-containing functional group includes hydroxyl, carboxyl, or a combination thereof; And / or, the nitrogen-containing functional group includes an amino group.
4. The battery separator according to claim 1, characterized in that, The mass ratio of the solid electrolyte to the binder is (5~10):1; And / or, the solid electrolyte comprises at least one of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, or lithium lanthanum zirconium oxide; And / or, the adhesive comprises at least one of polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, polyethylene oxide, sodium alginate, polytetrafluoroethylene, polyvinylpyrrolidone, polyacrylonitrile, or polyvinyl alcohol.
5. The battery separator according to claim 1, characterized in that, The pore size of the base film is 0.1~1μm; And / or, the material of the base film is selected from polyolefins.
6. A method for preparing a battery separator, characterized in that, Includes the following steps: A solid electrolyte and a binder are dispersed in a solvent to form a slurry; active functional groups are introduced into the slurry to form a modified slurry, wherein the active functional groups include oxygen-containing functional groups and nitrogen-containing functional groups; The modified slurry is applied to the surface of the base film, dried, and rolled to obtain the battery separator as described in any one of claims 1 to 5.
7. The preparation method according to claim 6, characterized in that, The active functional groups are introduced by means of plasma treatment, chemical grafting treatment, or a combination thereof.
8. The preparation method according to claim 7, characterized in that, The processing gases for plasma treatment include oxygen and nitrogen; And / or, the processing power of the plasma treatment is 100~200W; And / or, the plasma treatment time is 1~10 min; And / or, the treatment reagent for the chemical grafting treatment includes a coupling agent; And / or, the chemical grafting treatment is performed at a temperature of 50~70℃; And / or, the chemical grafting treatment takes 1 to 3 hours.
9. A battery, characterized in that, The battery includes a battery separator as described in any one of claims 1 to 5.
Citation Information
Patent Citations
Preparation method of modified separator for lithium ion battery
CN109119573A
Lithium battery diaphragm with gradient pore structure and preparation method thereof
CN119812677A
Microporous diaphragm for low-electrical-impedance lithium battery and preparation method of microporous diaphragm