Negative electrode active materials and preparation methods, negative electrode sheets, secondary batteries, and electrical equipment.

By granulating and graphitizing needle-shaped coke primary particles with fused-ring amide polymers, a high-capacity negative electrode active material is formed, solving the problem of binders affecting battery capacity and improving battery performance and fast charging performance.

CN121376998BActive Publication Date: 2026-11-10SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511433514.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-09-30
Publication Date
2026-11-10
Estimated Expiration
2045-09-30

AI Technical Summary

Technical Problem

In existing technologies, the addition of binders affects the capacity of secondary batteries, making it difficult to maintain high battery capacity while improving electrochemical performance.

Method used

A high-capacity negative electrode active material is prepared by granulating needle-shaped coke particles with an amide polymer having a fused ring structure, and by the bonding effect of the amide polymer with a fused ring structure and graphitization treatment.

Benefits of technology

It increases the capacity of the negative electrode active material, improves battery performance, reduces the impact of binder addition on battery capacity, and enhances the battery's fast charging performance and initial efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121376998B_ABST
    Figure CN121376998B_ABST
Patent Text Reader

Abstract

This application discloses a negative electrode active material and its preparation method, a negative electrode sheet, a secondary battery, and an electrical device. The preparation method of the negative electrode active material includes: granulating needle-shaped coke primary particles with an amide polymer having a fused ring structure to obtain a graphite particle precursor; and graphitizing the graphite particle precursor to obtain the negative electrode active material; wherein the amide polymer with the fused ring structure forms a granulated layer after graphitization. The beneficial effects of this application are: it provides a method for granulating needle-shaped coke primary particles with an amide polymer having a fused ring structure. On the one hand, the amide polymer with the fused ring structure has a binding effect, causing the needle-shaped coke primary particles to bond together to form larger particles; on the other hand, the amide polymer with the fused ring structure forms a graphite layered granulated layer after graphitization, resulting in a negative electrode active material with higher capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of new energy technology, and in particular relates to a negative electrode active material and its preparation method, a negative electrode sheet, a secondary battery, and electrical equipment. Background Technology

[0002] The negative electrode of a battery is a crucial component, responsible for storing and releasing electrical energy. The performance of the negative electrode directly impacts the overall performance of the battery.

[0003] In some related technologies, using binders to improve the granulation degree of graphite can optimize process performance and enhance electrochemical performance.

[0004] However, the addition of binders can affect battery capacity. Summary of the Invention

[0005] In view of this, this application provides a negative electrode active material and preparation method, a negative electrode sheet, a secondary battery, and an electrical device, aiming to solve the technical problem of secondary battery capacity.

[0006] As a first aspect of this application, an embodiment of this application provides a method for preparing a negative electrode active material, the preparation method comprising: The needle-shaped coke particles are granulated with an amide polymer having a fused ring structure to obtain a graphite particle precursor containing a granulation layer. The graphite particle precursor is graphitized to obtain the negative electrode active material.

[0007] Optionally, in some embodiments of this application, the method for preparing the amide polymer with a fused ring structure includes: performing a condensation reaction between a diacid anhydride with a fused ring structure and an aromatic diamine to obtain an amide polymer with a fused ring structure.

[0008] Optionally, in some embodiments of this application, the Dv50 value of the needle coke primary particles ranges from 9 μm to 12 μm.

[0009] Optionally, in some embodiments of this application, the dicarboxylic acid anhydride with a fused ring structure includes one or more of perylenetetracarboxylic dianhydride and pyromellitic dianhydride.

[0010] Optionally, in some embodiments of this application, the aromatic diamine includes one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, terephthalamide, and 1,5-diaminonaphthalene.

[0011] Optionally, in some embodiments of this application, the solid content of the amide polymer having a fused ring structure ranges from 16% to 25%.

[0012] Optionally, in some embodiments of this application, the carbon residue of the amide polymer having a fused ring structure ranges from 55% to 65%.

[0013] Optionally, in some embodiments of this application, the amount of the amide polymer with the fused ring structure added is positively correlated with the residual carbon content of the granulation layer, wherein the residual carbon content of the granulation layer ranges from 0.8% to 2.0%.

[0014] Optionally, in some embodiments of this application, the graphitization treatment of the graphite particle precursor includes: the heating rate is in the range of 2℃ / min to 5℃ / min.

[0015] Optionally, in some embodiments of this application, the treatment is carried out for 2 to 5 hours in the range of 1300°C to 1800°C.

[0016] Optionally, in some embodiments of this application, the treatment is carried out in the range of 1800°C to 2400°C for 2 hours to 5 hours, and then kept at 2100°C to 2200°C for 2 hours.

[0017] Optionally, in some embodiments of this application, the treatment is carried out in the range of 2400°C to 2800°C for 2 to 5 hours.

[0018] Optionally, in some embodiments of this application, the treatment is carried out in the range of 2800°C to 3000°C for 1 to 3 hours, and then kept at 3000°C to 3100°C for 3 hours.

[0019] Optionally, in some embodiments of this application, the granulation process of the needle coke primary particles and the amide polymer with a fused ring structure includes: mixing the needle coke primary particles, the amide polymer with a fused ring structure, and a solvent under preset mixing conditions to obtain a mixed raw material; carbonizing the mixed raw material under preset carbonization conditions to obtain a carbonized product; and coating the carbonized product with an adhering material to form a coating layer to obtain a graphite particle precursor.

[0020] Optionally, in some embodiments of this application, the solvent is one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide.

[0021] The preset mixing conditions include: a mixing temperature ranging from 25°C to 50°C, a mixing speed ranging from 500 rpm to 700 rpm, and a mixing time ranging from 10 min to 30 min.

[0022] Optionally, in some embodiments of this application, the preset mixing process includes one or more of fusion mixing granulation and spheroidizing mixing granulation.

[0023] Optionally, in some embodiments of this application, the coating process includes one or more of liquid phase spray coating and liquid phase fusion coating.

[0024] Optionally, in some embodiments of this application, the preset carbonization conditions include: The protective gas for carbonization includes one or more of nitrogen or argon; the heating rate ranges from 1℃ / min to 2℃ / min.

[0025] The heating rate from 200°C to 600°C is 1°C / min to 2°C / min, wherein the temperature is held at 400°C to 500°C for 1 hour; and / or, the heating rate from 600°C to 1000°C is 1°C / min to 2°C / min, wherein the temperature is held at 700°C to 800°C for 1 hour; and / or, the heating rate from 1000°C to 1250°C is 1°C / min to 2°C / min, wherein the temperature is held at 1150°C to 1250°C for 2 hours.

[0026] Optionally, in some embodiments of this application, the solvent includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide.

[0027] Optionally, in some embodiments of this application, the residual carbon content of the coating layer ranges from 0.1% to 0.5%.

[0028] Optionally, in some embodiments of this application, the attachment comprises a polymeric material having a fused ring structure, wherein the polymeric material includes , One or more of the -NH-CO- groups; wherein, Indicates the connection site.

[0029] Optionally, in some embodiments of this application, the attachment comprises the amide polymer having a fused ring structure.

[0030] As a second aspect of this application, embodiments of this application provide a negative electrode active material, including a negative electrode active material prepared by the preparation method described above.

[0031] As a third aspect of this application, embodiments of this application provide a negative electrode sheet, including the negative electrode active material as described above or the negative electrode active material prepared by the aforementioned preparation method.

[0032] Optionally, in some embodiments of this application, the value of the negative electrode active material ranges from 14 μm to 20 μm.

[0033] Optionally, in some embodiments of this application, the peak intensity ratio ID / IG(A) of the negative electrode active material ranges from 0.056 to 0.108.

[0034] As a fourth aspect of this application, embodiments of this application provide a secondary battery, including the negative electrode as described above.

[0035] As a fifth aspect of this application, embodiments of this application provide an electrical device including the secondary battery as described above.

[0036] The beneficial effects of this application are as follows: It provides a method for granulating needle-shaped coke primary particles with an amide polymer having a fused ring structure. On the one hand, the amide polymer with a fused ring structure has an adhesive effect, causing the needle-shaped coke primary particles to bond together to form larger particles. On the other hand, the amide polymer with a fused ring structure forms a granulation layer through graphitization treatment. The amide polymer with a fused ring structure has a fused ring structure, and it is easy to form a graphite layer structure during the graphitization process, resulting in a higher capacity of the prepared negative electrode active material, thereby improving the battery performance. The application also provides a negative electrode active material, a preparation method, a negative electrode sheet, a secondary battery, and electrical equipment. Attached Figure Description

[0037] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0038] Figure 1 This is a schematic diagram of the main steps of the preparation method provided by some embodiments of this application; Figure 2 This is a TEM image of the negative electrode active material in Example 2 of this application; Figure 3 This is a SEM image of the negative electrode active material in Example 2 of this application. Detailed Implementation

[0039] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In addition, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0041] In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish a numerical order.

[0042] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.

[0043] In this application, "at least one" means one or more, and "more than one" means two or more. "One or more", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0044] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0045] As a first aspect, such as Figure 1 As shown in the embodiment of this application, a method for preparing a negative electrode active material is provided, the preparation method comprising: Step S100: The needle-shaped coke primary particles are granulated with an amide polymer having a fused ring structure to obtain a graphite particle precursor containing a granulation layer. Step S200: The graphite particle precursor is graphitized to obtain the negative electrode active material.

[0046] It is understandable that granulation of needle-shaped coke primary particles using amide polymers with fused-ring structures involves two main processes. Firstly, the amide polymers with fused-ring structures act as binders, causing the needle-shaped coke primary particles to bond and form larger particles. Secondly, the amide polymers with fused-ring structures form a granulation layer through graphitization. The fused-ring structure of the amide polymers facilitates the formation of graphite layered structures during graphitization, resulting in a higher capacity for the prepared negative electrode active material. In some embodiments of this application, the method for preparing the amide polymer with a fused ring structure includes: performing a condensation reaction between a diacid anhydride with a fused ring structure and an aromatic diamine to obtain an amide polymer with a fused ring structure.

[0047] It is understandable that amide polymers with fused-ring structures are obtained by the condensation reaction of diacid anhydrides and aromatic diamines with fused-ring structures. They are coplanarly linked by imide bonds, with each repeating unit containing two benzene rings and two imide rings. The main chain is linear, eliminating molecular kinks and reducing steric hindrance. At high temperatures, they directly stack to form an AB graphite layered structure, generating large-sized graphite microcrystals. Simultaneously, the condensed-ring structure of the diacid anhydride and aromatic diamine is liquid, allowing the solvent to fully wet the surface of the primary needle coke particles, achieving initial adsorption through hydrogen bonding and π-π interactions. The high permeability of the solution allows it to fill the gaps between the primary needle coke particles, forming a "physical cross-linked network" after drying. The active functional groups on the granulator surface and the primary needle coke particles form strong interfacial interactions through hydrogen bonds, π-π stacking, and dipole forces. During cross-linking curing and heat treatment carbonization, efficient bonding is further achieved through chemical bonding and mechanical interlocking, thus achieving the purpose of granulating the primary needle coke particles into secondary particles. Compared to asphalt and phenolic resin granulators, this method can reduce the amount of granulator required, thereby improving the capacity utilization of the negative electrode active material.

[0048] In some embodiments of this application, the Dv50 value of the needle coke primary particles ranges from 9 μm to 12 μm. The Dv50 value of the needle coke primary particles includes any value of 9 μm, 10 μm, 11 μm, and 12 μm, or an interval of any two values.

[0049] Understandably, the Dv50 of needle coke primary particles is crucial for balancing battery capacity and processing performance. When the specific surface area of ​​needle coke primary particles increases dramatically, more electrolyte is consumed during charge / discharge to form a thicker SEI film, resulting in low initial efficiency and significant capacity loss. Simultaneously, the low tap density of small particles leads to a lower electrode volumetric energy density. When the Dv50 of needle coke primary particles is too large, the diffusion path of lithium ions within the particles becomes longer, deteriorating rate performance. Furthermore, large particles are prone to scratches during coating, affecting electrode quality uniformity and worsening processing performance.

[0050] In some embodiments of this application, the dicarboxylic anhydride having a fused ring structure includes one or more of perylene tetracarboxylic dianhydride (PTCDA) and pyromellitic tetracarboxylic dianhydride (PMDA).

[0051] In some embodiments of this application, the aromatic diamine includes one or more of 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (PDA), terephthalamide (TA), and 1,5-diaminonaphthalene (NDA).

[0052] It is understandable that condensation reactions between diacid anhydrides with fused ring structures and aromatic diamines yield amide polymers with fused ring structures. These polymers are coplanarly linked by imide bonds, with each repeating unit containing two benzene rings and two imide rings. The main chain is linear, eliminating molecular kinks and reducing steric hindrance. At high temperatures, they are directly stacked into AB graphite layered structures, generating large-sized graphite microcrystals.

[0053] In some embodiments of this application, the solid content of the amide polymer having a fused ring structure ranges from 16% to 25%.

[0054] It is understood that the solid content of the amide polymer with a fused ring structure can be any value or a range of any two values ​​from 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, or 25%. Within this range, the solid content of the amide polymer with a fused ring structure allows the solvent to fully wet the surface of the needle-shaped coke primary particles, achieving initial adsorption through hydrogen bonding, π-π interactions, etc.

[0055] In some embodiments of this application, the carbon residue rate of the amide polymer with a fused ring structure ranges from 55% to 65%. The carbon residue rate of the amide polymer with a fused ring structure can be any value or a range of any two of the following: 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, or 65%. In this application, the carbon residue rate is the percentage of residual carbon remaining after incomplete combustion or decomposition of the polymer material in an inert gas (such as nitrogen) atmosphere at high temperature, relative to the initial sample mass. The carbon residue rate is calculated using thermogravimetric analysis (TGA) by monitoring the mass loss curve of the sample under nitrogen atmosphere as it heats from room temperature to 1000°C, with a heating rate of 10°C / min.

[0056] In some embodiments of this application, the amount of the amide polymer with a fused ring structure added is positively correlated with the residual carbon content of the granulation layer. The residual carbon content of the granulation layer ranges from 0.8% to 2.0%.

[0057] It is understandable that the residual carbon content of the granulation layer can range from any value or any two values ​​within the ranges of 0.8%, 0.9%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, and 2.0%. The ratio of the mass of the amide polymer with a fused ring structure to the mass of the needle-shaped coke primary particles = residual carbon content of the granulation layer / (solid content of the amide polymer with a fused ring structure). (Carbon residue of amide polymers with fused ring structures). The addition of amide polymers with fused ring structures allows for the preparation of secondary particles from primary particles through granulation. The construction of secondary particles shortens the lithium-ion diffusion path, reduces electrode tortuosity and ion transport resistance, thereby improving fast-charging performance. When too little granulating agent is added, the granulation degree is low, failing to achieve the granulation effect of graphite particles. The lithium-ion diffusion path is long and the ion transport resistance is high, resulting in low fast-charging performance. When the amount of granulating agent added is too high, the graphite particle size is too large, resulting in poor processing performance and difficulty in application.

[0058] In some embodiments of this application, the graphitization treatment of the graphite particle precursor includes a heating rate ranging from 2°C / min to 5°C / min.

[0059] It is understandable that the heating rate can be any value or any two values ​​from 2℃ / min, 3℃ / min, 4℃ / min, and 5℃ / min.

[0060] In some embodiments of this application, the treatment is carried out at a temperature between 1300°C and 1800°C for 2 to 5 hours.

[0061] In some embodiments of this application, the treatment is carried out in the range of 1800°C to 2400°C for 2 to 5 hours, and then kept at 2100°C to 2200°C for 2 hours.

[0062] In some embodiments of this application, the treatment is carried out in the range of 2400°C to 2800°C for 2 to 5 hours.

[0063] In some embodiments of this application, the treatment is carried out in the range of 2800°C to 3000°C for 1 to 3 hours, and then kept at 3000°C to 3100°C for 3 hours.

[0064] Understanding this process involves processing at 1300°C to 1800°C for 2 to 5 hours to further eliminate volatiles, allowing the graphite layer to gradually form and the particle size to increase. Excessive temperature at this stage disrupts the growth pattern of graphite microcrystals, leading to high structural disorder; conversely, insufficient temperature results in a high proportion of sp³ hybrid carbon. The optimal heating rate at this stage is 2°C / min to 5°C / min. Excessive heating will cause carbon layer distortion, a high proportion of sp³ hybrid carbon, and a significant increase in specific surface area; insufficient heating results in an excessively long development process, high cost, and low efficiency.

[0065] The process involves treating the graphite layers at 1800°C to 2400°C for 2 to 5 hours, followed by a 2200°C hold-up period. During this stage, elongated, graphite-stacked planar layers are formed. Excessive temperature disrupts the growth of graphite crystallites, leading to high structural disorder; conversely, insufficient temperature results in low graphitization. A heating rate of 2°C / min to 5°C / min during this stage promotes the ordering of the graphite crystal structure and increases the proportion of sp² hybridized carbon. Excessive heating rate distorts the carbon layers, resulting in a high proportion of sp³ hybridized carbon and a significantly increased specific surface area; conversely, a low heating rate leads to excessively long processing times, high costs, and low efficiency.

[0066] The process involves treating the graphite layers at 2400°C to 2800°C for 2 to 5 hours, during which the graphite layers gradually grow and stack. Excessive temperature disrupts the growth pattern of graphite crystallites, leading to high structural disorder; excessively low temperature results in low graphitization. A heating rate of 2°C / min to 5°C / min during this stage promotes the ordered structure of the graphite crystals and increases the proportion of sp² hybrid carbon. Excessively high heating rates distort the carbon layers, resulting in a high proportion of sp³ hybrid carbon and a significantly increased specific surface area; conversely, excessively low rates lead to excessively long processing times, high costs, and low efficiency.

[0067] The graphite is treated at 2800°C to 3000°C for 1 hour, followed by a hold at 3000°C to 3100°C for 3 hours. During this stage, graphite recrystallizes, further increasing its graphitization degree. Due to equipment limitations, the graphitization temperature is generally limited to a maximum of 3000°C. If the temperature is too low during this stage, the graphitization of the graphite particles will be insufficient. The heating rate during this stage is 2°C / min to 5°C / min, which is beneficial for the ordered structure of the graphite crystals and increases the proportion of sp² hybrid carbon. If the heating rate is too high, the carbon layers will be distorted, resulting in a high proportion of sp³ hybrid carbon and a significantly increased specific surface area; if the rate is too low, the recrystallization degree of graphite will be poor, and the graphitization degree will be low.

[0068] In some embodiments of this application, the granulation process of needle-shaped coke primary particles with an amide polymer having a fused ring structure includes: mixing the needle-shaped coke primary particles, the amide polymer having a fused ring structure, and a solvent under preset mixing conditions to obtain a mixed raw material; carbonizing the mixed raw material under preset carbonization conditions to obtain a carbonized product; and coating the carbonized product with an adhering material to form a coating layer to obtain a graphite particle precursor.

[0069] like Figure 2 As shown in the TEM image of the negative electrode active material in Example 2 of the present invention, the coating layer of the negative electrode active material can be seen.

[0070] Understandably, carbonizing the mixed raw materials under preset carbonization conditions aims to promptly determine the morphology of the carbonized product and eliminate primary needle-like coke particles and light components in amide polymers with fused ring structures, which is beneficial for subsequent graphitization processes. If carbonization is performed after coating, it may result in high volatile matter content and poor surface structure, thus affecting the initial efficiency.

[0071] Understandably, a small amount of deposits coated and graphitized can reduce surface defects, improve surface density, and thus improve the first-effect index.

[0072] In some embodiments of this application, the solvent is one or more of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), and N,N-dimethylformamide (DMF).

[0073] The preset mixing conditions include: a mixing temperature ranging from 25°C to 50°C, a mixing speed ranging from 500 rpm to 700 rpm, and a mixing time ranging from 10 min to 30 min.

[0074] Understandably, the mixing temperature can be any value or any two values ​​within the range of 25℃, 30℃, 35℃, 40℃, 45℃, or 50℃. Excessively high mixing temperatures will affect the bonding effect, resulting in low granulation degree. The mixing speed can be any value or any two values ​​within the range of 500rpm, 550rpm, 600rpm, 650rpm, or 700rpm. Within this range, the granulation degree and bonding strength of the graphite particles are good, and the particle size meets the requirements, thus improving fast-charging performance. When the speed is too low, the stirring time is too short, resulting in insufficient mixing, low granulation degree and bonding strength, substandard particle size, and low fast-charging performance. Excessively high speed and excessively long stirring time will damage the structure of the graphite particles, leading to particle dissociation and breakage, thus affecting the initial effect. The mixing time can be any value or any two values ​​within the range of 10min, 15min, 20min, 25min, or 30min.

[0075] In some embodiments of this application, the preset mixing process includes one or more of fusion mixing granulation and spheroidizing mixing granulation.

[0076] In some embodiments of this application, the coating process includes one or more of liquid phase spray coating and liquid phase fusion coating.

[0077] In some embodiments of this application, the preset carbonization conditions include: The protective gas for carbonization includes one or more of nitrogen or argon; the heating rate ranges from 1℃ / min to 2℃ / min.

[0078] The heating rate from 200°C to 600°C is 1°C / min to 2°C / min, wherein the temperature is held at 400°C to 500°C for 1 hour; and / or, the heating rate from 600°C to 1000°C is 1°C / min to 2°C / min, wherein the temperature is held at 700°C to 800°C for 1 hour; and / or, the heating rate from 1000°C to 1250°C is 1°C / min to 2°C / min, wherein the temperature is held at 1150°C to 1250°C for 2 hours.

[0079] Understandably, during the carbonization furnace temperature range of 200℃ to 600℃, adsorbed water and residual solvents in the mixed raw materials volatilize, molecular chains and functional groups break, producing small molecules such as H2O, CH4, and HCN, and releasing CO and CO2. During the heating phase within this range, if the temperature is too high or the heating rate is too rapid, significant molecular chain breakage will occur. This molecular chain stacking leads to material embrittlement, affecting granulation bonding strength and causing a decrease in capacity, initial efficiency, and rate performance. In the 600℃ to 1000℃ range, the structure transitions from polymer to amorphous carbon. Residual aromatic rings undergo dehydrogenation and condensation to form polycyclic aromatic hydrocarbon structures. Free radical reactions lead to cross-linking of the carbon skeleton, generating graphite-like microregions. In the 1000℃ to 1250℃ range, the mixed raw materials undergo further aromatization and dehydrogenation, carbon microcrystals become ordered, the proportion of sp² hybrid carbon increases, and a graphite-like carbonized product is gradually formed. If the temperature rises too quickly during the temperature rise phase after exceeding 700℃, it will affect the aromatic heterocyclic condensation reaction in aromatization, resulting in the flatness of the two-dimensional planar condensed heterocycles, which in turn will affect the subsequent formation of the graphite layered structure.

[0080] In some embodiments of this application, the solvent includes one or more of N,N-dimethylacetamide (DMF), N-methylpyrrolidone (NMP), and N,N-dimethylformamide (DMAc).

[0081] In some embodiments of this application, the residual carbon content of the coating layer ranges from 0.1% to 0.5%.

[0082] It is understood that the residual carbon content of the coating layer can be any value or a range of any two values, such as 0.2%, 0.3%, 0.4%, and 0.5%. This application uses an amide polymer with a fused ring structure as the adhesive to form the coating layer. The ratio of the mass of the adhesive to the graphite particles = residual carbon content of the coating layer / (solid content of the adhesive). (Carbon residue rate of the adhering material). The carbon residue rate of the coating layer is set according to actual needs. An increase in the carbon residue rate of the coating layer indicates an increase in the amount of amide polymer with a fused ring structure added to the surface of the graphite particles. An increase in the thickness of the coating layer can optimize the electronic structure of the coating layer and graphitize it, which can reduce surface defects and improve surface density. The effect is mainly reflected in Raman ID / IG and first-effect index.

[0083] In some embodiments of this application, the attachment comprises a polymeric material having a fused ring structure, wherein the polymeric material includes , One or more of the -NH-CO- groups; the molecular weight of the polymer material ranges from 10,000 to 20,000. Indicates the connection site.

[0084] In some embodiments of this application, the attachment includes one or more of the amide polymer having a fused ring structure and polyoxadiazole.

[0085] As a second aspect of this application, embodiments of this application provide a negative electrode active material, including a negative electrode active material prepared by the preparation method described above. Figure 3 This is a SEM image of the negative electrode active material in Example 2 of the present invention.

[0086] As a third aspect of this application, embodiments of this application provide a negative electrode sheet, including the negative electrode active material as described above or the negative electrode active material prepared by the aforementioned preparation method.

[0087] In some embodiments of this application, the value of the negative electrode active material ranges from 14 μm to 20 μm.

[0088] It is understandable that the value range of the negative electrode active material includes any value or any two values ​​from 14, 15, 16.2, 16.8, 17, 17.4, 17.5, 17.6, 17.8, 18, 18.5, 18.8, 19.5, 19.8, and 20.

[0089] In some embodiments of this application, the peak intensity ratio ID / IG(A) of the negative electrode active material ranges from 0.056 to 0.108.

[0090] It is understandable that the peak intensity ratio ID / IG(A) of the negative electrode active material can take any value or any two values ​​within the range of 0.056, 0.06, 0.061, 0.062, 0.063, 0.064, 0.065, 0.066, 0.067, 0.068, 0.069, 0.07, 0.077, 0.078, 0.08, 0.081, 0.082, 0.085, 0.089, 0.09, 0.091, 0.095, 0.098, 0.099, and 0.108.

[0091] In some embodiments of this application, the particle size distribution span value (D90-D10) / D50 of the negative electrode active material is <1.5.

[0092] As a fourth aspect of this application, embodiments of this application provide a secondary battery, including the negative electrode as described above.

[0093] As a fifth aspect of this application, embodiments of this application provide an electrical device including the secondary battery as described above.

[0094] The present application will be further described below through specific embodiments.

[0095] Example 1 S11: The needle coke raw material is calcined at above 1400℃ for 8 hours, then coarsely crushed, mechanically ground and graded and shaped, and screened to obtain needle coke primary particles with Dv50 of 10 microns. S12: Take 30 kg of needle-shaped coke particles with a Dv50 of 9 μm and put them into a liquid phase coating fusion machine and stir at a low speed of 100 rpm; S13: According to the granulation layer residual carbon rate of 1.2%, slowly add 3.75 kg of polyamic acid (synthesized from PMDA:ODA=1:1, with a solid content of 16% and a carbon residual rate of 60%); stir for 10 min to mix it. S14: Circulate water, maintain the temperature at 25℃, mix at 600 rpm, and stir for 20 minutes to obtain the mixed raw materials; S15: Place the obtained mixed raw materials in a carbonization furnace, and heat from room temperature under nitrogen protection at a flow rate of 10 L / min. In the range of 200℃ to 600℃, heat at a heating rate of 2℃ / min for 3.5 h, and hold at 500℃ for 1 h; in the range of 600℃ to 1000℃, heat at a heating rate of 2℃ / min for 3.5 h, and hold at 800℃ for 1 h; in the range of 1000℃ to 1250℃, heat at a heating rate of 2℃ / min for 2 h, and hold at 1250℃ for 2 h to obtain the carbonized product.

[0096] S16: The carbonized product obtained in S15 is subjected to graphitization treatment to obtain the negative electrode active material. Using a medium-frequency furnace high-temperature graphitization furnace, the obtained coated product is treated under argon protection at an argon flow rate of 5 L / min and a heating rate of 5 °C / min for 2 hours in the range of 1300 °C to 1800 °C; 5 hours in the range of 1800 °C to 2400 °C; 2 hours at 2100 °C to 2200 °C; 4 hours in the range of 2400 °C to 2800 °C; 1 hour in the range of 2800 °C to 3000 °C; and 3 hours at 3000 °C, thus obtaining the negative electrode active material.

[0097] In this embodiment, ODA (4.2 mol) was added to deionized water (8.4 kg), and a small amount of hydrochloric acid was added to adjust the pH to 2-3. The mixture was stirred until completely dissolved. PMDA (4.2 mol) was added to the ODA solution in batches (dropping rate 1 g / min), and the temperature was controlled at 40°C. Stirring was continued (40°C to 50°C, 6-12 hours) to induce polycondensation and generate polyamic acid. Triethylamine (TEA, 5 mol) was then added to form an aqueous polyimide slurry. The imidized solution was transferred to a vacuum degassing tank (-0.09 MPa, 25°C) to remove air bubbles. The solution was then filtered through a 1-5 μm filter membrane and stored at 5-10°C under sealed conditions.

[0098] In the embodiments of this application, the synthesis steps of other polyamic acids are the same as those in this embodiment, only the raw materials are replaced accordingly.

[0099] Example 2 The difference between this embodiment and Embodiment 1 is that step 7 is added after step 6; step 7 in Embodiment 1 is step 8. The specific steps are as follows: S21: The needle coke raw material is calcined at above 1400℃ for 8 hours, then coarsely crushed, mechanically ground and graded and shaped, and screened to obtain needle coke primary particles with Dv50 of 10 microns. S22: Take 30 kg of needle-shaped coke particles with a Dv50 of 9 μm and put them into a liquid phase coating fusion machine and stir at a low speed of 100 rpm; S23: According to the granulation layer residual carbon rate of 1.2%, slowly add 3.75 kg of polyamic acid (synthesized from PMDA:ODA=1:1, with a solid content of 16% and a carbon residual rate of 60%); stir for 10 min to mix it. S24: Circulate water, maintain the mixing temperature at 25℃, mix at 600 rpm, and stir for 20 minutes to obtain the mixed raw materials; S25: Place the obtained mixed raw materials in a carbonization furnace, and heat from room temperature under nitrogen protection at a flow rate of 10 L / min. In the range of 200℃ to 600℃, heat at a heating rate of 2℃ / min for 3.5 h, and hold at 500℃ for 1 h; in the range of 600℃ to 1000℃, heat at a heating rate of 2℃ / min for 3.5 h, and hold at 800℃ for 1 h; in the range of 1000℃ to 1250℃, heat at a heating rate of 2℃ / min for 2 h, and hold at 1250℃ for 2 h to obtain the carbonized product.

[0100] S26: Add 30kg of the shaped product to a planetary mixer. Weigh 625g of polyamic acid (synthesized from PMDA:ODA=1:1, with a solid content of 16% and a carbon residue rate of 60%) according to the residual carbon rate of the attached material of 0.2%. Stir for 30 minutes to mix the materials. Transfer the suspension to a spray plate using a peristaltic pump. Set the speed of the centrifugal spray plate to 13000rpm, the spray inlet temperature to 240℃, and the outlet temperature to 120℃. Obtain the graphite particle precursor by centrifugal spray coating. S27: The graphite particle precursor obtained in S26 is graphitized to obtain the negative electrode active material. Using a medium-frequency furnace high-temperature graphitization furnace, the obtained coated product is treated under argon protection at a flow rate of 5 L / min and a heating rate of 5 °C / min, within the range of 1300 °C to 1800 °C for 2 hours; within the range of 1800 °C to 2400 °C for 5 hours; held at 2100 °C to 2200 °C for 2 hours; within the range of 2400 °C to 2800 °C for 4 hours; within the range of 2800 °C to 3000 °C for 1 hour; and held at 3000 °C for 3 hours, thus obtaining the negative electrode active material. Figure 3 As shown, the surface of the particles is covered with an ordered graphite structure.

[0101] Example 3 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 0.4%, which means that 1.25 kg of polyamic acid is added.

[0102] Example 4 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 0.8%, which means that 2.50 kg of polyamic acid is added.

[0103] Example 5 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 1.4%, which means that 4.375 kg of polyamic acid is added.

[0104] Example 6 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 1.6%, which means that 5.0 kg of polyamic acid is added.

[0105] Example 7 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 1.8%, which means that 5.625 kg of polyamic acid is added.

[0106] Example 8 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 2.0%, which means that 6.25 kg of polyamic acid is added.

[0107] Example 9 The difference from Example 2 is that the residual carbon rate of the granulation layer in S23 is 2.2%, which means that 6.875 kg of polyamic acid is added.

[0108] Example 10 The difference from Example 2 is that the granulating agent in S23 is 3.75 kg of polyamic acid (PTCDA:TA=1:1 synthesized, with a solid content of 16% and a carbon residue rate of 60%).

[0109] Example 11 The difference from Example 2 is that the granulating agent in S23 is 3.75 kg of polyamic acid (PTCDA:NDA = 1:1 synthesized, with a solid content of 16% and a carbon residue rate of 60%).

[0110] Example 12 The difference from Example 2 is that the residual carbon rate of the coating layer in S26 is 0.05%, that is, 156.25g of polyamic acid is added as an adhering material.

[0111] Example 13 The difference from Example 2 is that the residual carbon rate of the coating layer in S26 is 0.1%, that is, 312.5g of polyamic acid is added as an adhering material.

[0112] Example 14 The difference from Example 2 is that the residual carbon rate of the coating layer in S26 is 0.3%, that is, 937.5g of polyamic acid is added as an adhering material.

[0113] Example 15 The difference from Example 2 is that the residual carbon rate of the coating layer in S26 is 0.4%, that is, 1250g of polyamic acid is added as an adhering material.

[0114] Example 16 The difference from Example 2 is that the residual carbon rate of the coating layer in S26 is 0.5%, that is, 1562.5g of polyamic acid is added as an adhering material.

[0115] Example 17 The difference from Example 2 is that the residual carbon rate of the coating layer in S26 is 0.7%, that is, 2187.5g of polyamic acid is added as an adhering material.

[0116] Example 18 The difference from Example 2 is that the adhering substance in S26 is polyamic acid (PTCDA:TA=1:1 synthesis, solid content of 16%, carbon residue rate of 60%), that is, 625g of polyamic acid is added as the adhering substance.

[0117] Example 19 The difference from Example 2 is that the adhering substance in S26 is polyamic acid (PTCDA:NDA=1:1 synthesis, solid content is 16%, carbon residue rate is 60%), that is, 625g of polyamic acid is added as the adhering substance.

[0118] Example 20 The difference from Example 2 is that the adhering substance in S26 is sulfonic acid-modified waterborne polyoxadiazole (solid content of 16% and carbon residue rate of 60%), that is, 625g of polyoxadiazole is added as the adhering substance.

[0119] Example 21 The difference from Example 2 is that the primary needle-shaped coke particles in S21 have a Dv50 of 8 μm.

[0120] Example 22 The difference from Example 2 is that the Dv50 of the needle-shaped coke primary particles in S21 is 9 μm.

[0121] Example 23 The difference from Example 2 is that the Dv50 of the needle-shaped coke primary particles in S21 is 11 μm.

[0122] Example 24 The difference from Example 2 is that the primary needle-shaped coke particles in S21 have a Dv50 of 12 μm.

[0123] Example 25 The difference from Example 2 is that the primary needle-shaped coke particles in S21 have a Dv50 of 13 μm.

[0124] Example 26 The difference from Example 2 is that the carbonization heating rate in S25 is 3°C / min.

[0125] Example 27 The difference from Example 2 is that the carbonization heating rate in S25 is 5°C / min.

[0126] Example 28 The difference from Example 2 is that the carbonization heating rate in S25 is 5°C / min, and the temperature is maintained at 1400°C for 2 hours.

[0127] Example 29 The difference from Example 2 is that the carbonization heating rate in S25 is 1℃ / min, and the temperature is maintained at 1000℃ for 2 hours.

[0128] Example 30 The difference from Example 2 is that the mixing temperature in S24 is 10°C.

[0129] Example 31 The difference from Example 2 is that the mixing temperature in S24 is 40°C.

[0130] Example 32 The difference from Example 2 is that the mixing temperature in S24 is 50°C.

[0131] Example 33 The difference from Example 2 is that the mixing temperature in S24 is 80°C.

[0132] Example 34 The difference from Example 2 is that the mixing speed in S24 is 500 rpm.

[0133] Example 35 The difference from Example 2 is that the mixing speed in S24 is 700 rpm.

[0134] Example 36 The difference from Example 2 is that the stirring time in S24 is 5 minutes and the mixing speed is 100 rpm.

[0135] Example 37 The difference from Example 2 is that the stirring time in S24 is 40 min and the mixing speed is 800 rpm.

[0136] Example 38 The difference from Example 2 is that the heating rate in S27 is 10°C / min.

[0137] Example 39 The difference from Example 2 is that S27 does not involve heat preservation at 2200°C.

[0138] Example 40 The difference from Example 2 is that the highest graphitization temperature in S27 is 2600°C.

[0139] Example 41 The difference from Example 2 is that the temperature is not maintained at 3000°C in S27.

[0140] Example 42 The difference from Example 2 is that there is no S25 granulation carbonization.

[0141] Comparative Example 1 The difference from Example 2 is that in S24, solid phase asphalt AYD250 from Liaoning Aoyida New Materials Co., Ltd. is used to granulate petroleum coke particles in a hot kettle, and the residual carbon rate of the granulation layer is 8%.

[0142] Comparative Example 2 The difference from Example 2 is that in S24, liquid resin is used for fusion granulation, and the residual carbon rate of the granulation layer is 4%.

[0143] Comparative Example 3 The difference from Example 2 is that in S24, aliphatic polyamic acid is used for mixing and granulation.

[0144] Comparative Example 4 The difference from Example 2 is that in S24, polyacrylic acid (PAA) is used for mixing and granulation.

[0145] Comparative Example 5 The difference from Example 2 is that in S24, phenolic resin is used for mixing and granulation.

[0146] Comparative Example 6 The difference from Example 2 is that the coating layer carbonization in S27 is not graphitized, that is, the graphitization process in S28 is changed to the carbonization process in S25.

[0147] Comparative Example 7 The difference from Example 2 is that the granulation and carbonization step in S25 is not performed, and only carbonization is performed after coating in S27. That is, the graphitization process in S27 is replaced by the carbonization process in S25.

[0148] Test methods Median particle size testing method: The particle size distribution range is tested using a Malvern MS3000 laser particle size analyzer with wet sample injection.

[0149] Raman spectroscopy measurements were performed using a Jobin Yvon LabRAM HR spectrometer with a 532 nm light source and a measurement range of 0 cm⁻¹. -1 ~4000cm -1 The testing range is 100μm. 100μm. Twenty-five anode material particles were randomly obtained and subjected to Raman spectroscopy. The results showed that the anode material at 1200 cm⁻¹... -1 ~1500cm -1 The peak area ID at 1500 cm⁻¹ is the same as that at 1500 cm⁻¹ -1 ~1800cm -1 The ratio of peak area IG at a given location, ID / IG, is Rn, where n = 1, 2, 3... 25; the average value of ID / IG for 25 composite anode material particles is R.

[0150] The preparation method of the button cell is as follows: The performance of the negative electrode materials in the examples and comparative examples was verified using a half-cell test method. The ratio of graphite:CMC:SP:SBR = 95:1.5:1.5:2 was used, and an appropriate amount of water was added to form a slurry. This slurry was then coated onto copper foil, and the coated electrode was placed in a vacuum drying oven at 110℃ for 4 hours for later use. The electrolyte was 1 mol / L LiPF6 / EC / DEC / DM, with lithium metal sheets as the counter electrode and a polypropylene microporous membrane as the separator. The cells were then assembled into a battery.

[0151] The testing method for button batteries is as follows: First-cycle capacity test: First, charge the battery at a constant current of 0.2C to 4.2V, then charge at a constant voltage to 10mA, and let it rest for 10 minutes. Then discharge it at a constant current of 0.2C to 2.7V, and let it rest for another 10 minutes. Repeat this charge-discharge cycle 3 times to obtain the battery capacity. First-cycle capacity is calculated as the ratio of the first charge capacity to the first discharge capacity.

[0152] Rate testing: The prepared coin cells were cycled 10 times each at 0.1C, 0.5C, 1C, 2C, and 0.1C. The 2C / 0.2C discharge capacity retention rate was calculated by dividing the 2C discharge capacity by the 0.2C discharge capacity. Table 1 shows the battery performance of the embodiments and comparative examples of this application.

[0153] Table 1. Characteristics of some raw materials in Examples 1 to 25 and Comparative Examples 1 to 5

[0154] Table 2 Test results of Examples 1 to 25 and Comparative Examples 1 to 5

[0155] Table 3. Process differences between Examples 26 to 42 and Comparative Examples 6 and 7

[0156] Table 4 Test results of Examples 26 to 41 and Comparative Examples 6 and 7

[0157] As can be seen from the comparison between Example 1 and Example 2, when there is a coating layer on the surface of the negative electrode active material, the defects on the surface of the negative electrode active material can be reduced, the surface density can be improved, and thus the first efficiency of the battery can be improved.

[0158] As can be seen from Examples 2 and Comparative Examples 1 to 5, the amide polymer with a fused ring structure used in this application as a granulator improves both capacity and initial efficiency. Comparative Example 1 and Example 2 have similar granulation levels, with particle size deviations of less than 1 micrometer after granulation. However, the comparative example uses a high amount of asphalt, which has a significant negative impact on the capacity of the negative electrode active material. Furthermore, due to its low degree of graphitization, surface defects are significantly increased, resulting in a decrease in capacity and initial efficiency.

[0159] As shown in Examples 3 and 9, when the residual carbon content of the granulation layer is in the range of 0.8% to 2%, the addition of amide polymers with fused ring structures allows the primary particles to be granulated into secondary particles. The construction of secondary particles shortens the lithium-ion diffusion path, reduces electrode tortuosity and ion transport resistance, thereby improving fast-charging performance. When too little granulating agent is added, the granulation degree is low, failing to achieve the granulation effect of graphite particles. The lithium-ion diffusion path is long and the ion transport resistance is high, resulting in low fast-charging performance. When the amount of granulating agent added is too high, the graphite particle size is too large, resulting in poor processing performance and difficulty in application.

[0160] The amide polymers with fused ring structures obtained from Examples 2, 10, and 11 using different raw materials all produced batteries with superior performance.

[0161] A comparison of Examples 2 and 12 to 17 shows that increasing the residual carbon content of the deposits and the thickness of the coating layer can optimize the electronic structure of the coating layer and promote graphitization, thereby reducing surface defects and improving surface density. The effects are mainly reflected in the Raman ID / IG ratio and the first-efficiency index. When the residual carbon content of the deposits is too low, the first-efficiency of the battery is reduced; when the residual carbon content of the deposits is too high, the particle size of the negative electrode active material is too large, resulting in poor processing performance.

[0162] As can be seen from Examples 2, 18 to 20, the attached material comprises a polymeric material with a fused ring structure, wherein the polymeric material includes , It contains one or more of the -NH-CO- groups. It can reduce defects on the surface of the negative electrode active material, improve surface density, and thus improve the battery's initial efficiency. Batteries with amide polymers having fused ring structures have higher initial efficiencies than those with asphalt or phenolic resins. The attached material contains fused ring structures and nitrogen-containing heterocycles, with alternating single and double bonds or large π bonds in the main chain. The large π bond density is high, and the aromatic rings are directly connected or connected through short bridge bonds. The aromatic rings are coplanarly arranged, exhibiting good planarity.

[0163] As shown in Examples 2 and 21 to 25, the Dv50 of the needle coke primary particles is crucial for balancing battery capacity and processing performance. When the specific surface area of ​​the needle coke primary particles increases dramatically, more electrolyte is consumed during charge and discharge to form a thicker SEI film, resulting in low initial efficiency and significant capacity loss. Simultaneously, the low tap density of small particles leads to a lower electrode volumetric energy density. When the Dv50 of the needle coke primary particles is too large, the diffusion path of lithium ions within the particles becomes longer, deteriorating rate performance. Furthermore, large particles are prone to scratches during coating, affecting electrode quality uniformity and worsening processing performance.

[0164] In Examples 26 and 27, the carbonization heating rate was too fast, which reduced the orderliness of the amide polymer with a fused ring structure as it transformed into a graphite layered structure, resulting in a decrease in battery capacity.

[0165] A comparison of Examples 2 with Examples 28 and 29 shows that in Example 28, the amide polymer with a fused ring structure exhibits poorer order in its conversion into a layered graphite structure, resulting in a decrease in battery capacity. In Example 29, the carbonization temperature after granulation was too low, leading to a poor graphite structure and a decline in performance.

[0166] A comparison of Examples 2 and Examples 30 to 33 shows that the mixing temperature during granulation is in the range of 25°C to 50°C. When the temperature is too low, the viscosity of the amide polymer with a fused ring structure is too high, resulting in poor flowability and poor granulation uniformity, which leads to a decrease in capacity. When the mixing temperature is too high, some substances in the amide polymer with a fused ring structure volatilize, the binder becomes weak, the degree of granulation is small, which also leads to a decrease in capacity.

[0167] A comparison of Examples 2 and Examples 33 to 37 shows that in Example 36, when the mixing speed is too low and the stirring time is short, the resulting negative electrode active material particles are small, the granulation uniformity is poor, and there is agglomeration, which affects the capacity utilization; in Example 37, the negative electrode active material D50 particles are small, and at high speed, the particles are subjected to a large degree of particle compression.

[0168] As demonstrated in Examples 2 and 38 to 41, the parameters related to the formation of the graphite particle precursor and the graphitization process significantly affect the performance of the negative electrode active material. Excessive graphitization heating rate can lead to carbon layer distortion, a high proportion of sp³ hybrid carbon, and a significantly increased specific surface area, ultimately impacting the battery's fast-charging performance. In Example 39, the lack of heat preservation at 2200℃ affected the formation of the graphite layered structure, ultimately impacting the battery's capacity and initial efficiency.

[0169] In Example 40, no heat preservation was performed at 2600°C. At this temperature, the graphite layered structure gradually grew and its stacking was affected, ultimately impacting the battery's capacity and initial efficiency.

[0170] In Example 41, the degree of graphitization of the negative electrode active material was affected because no heat preservation was performed at 3000℃, which ultimately affected the battery capacity and first-time efficiency.

[0171] Comparing Example 2 with Example 42 and Comparative Example 7, Example 42 did not undergo carbonization after granulation but was coated with an adsorbent. After coating, graphitization was performed. The amide polymer with a fused ring structure was not carbonized in time, and its morphology was not fixed promptly, potentially leading to high volatile content and poor surface structure, thus resulting in initial failure. The difference between Comparative Example 7 and Example 42 is that Comparative Example 7 only underwent carbonization after coating, without carbon graphitization, resulting in inferior performance compared to Example 42.

[0172] As can be seen from the comparison between Example 2 and Comparative Example 6, when carbonization is performed but graphitization is not carried out after coating treatment of carbonized products, the capacity, initial efficiency and rate of the battery are all affected.

[0173] The technical solutions provided by the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A method for preparing a negative electrode active material, characterized in that, The preparation method includes: Under preset mixing conditions, needle-shaped coke primary particles, amide polymers with fused ring structures, and solvents are mixed to obtain a mixed raw material; The mixed raw materials are carbonized under preset carbonization conditions to obtain carbonized products; The carbonized products are coated with an adhering material to form a coating layer, thereby obtaining a graphite particle precursor. The graphite particle precursor is graphitized to obtain the negative electrode active material. The amide polymer with a fused ring structure is graphitized to form a granulation layer. The amount of the amide polymer with a fused ring structure added is positively correlated with the residual carbon content of the granulation layer, wherein the residual carbon content of the granulation layer ranges from 0.8% to 2.0%.

2. The preparation method according to claim 1, characterized in that, The method for preparing the amide polymer with a fused ring structure includes: A condensation reaction is carried out between a diacid anhydride with a fused ring structure and an aromatic diamine to obtain an amide polymer with a fused ring structure.

3. The preparation method according to claim 2, characterized in that, The Dv50 value of the needle-shaped coke primary particles ranges from 9 μm to 12 μm; The dicarboxylic acid anhydride with a fused ring structure includes one or more of perylene tetracarboxylic dianhydride and pyromellitic tetracarboxylic dianhydride; And / or, the aromatic diamine includes one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, terephthalamide, and 1,5-diaminonaphthalene; And / or, the solid content of the amide polymer having a fused ring structure ranges from 16% to 25%; And / or, the carbon residue of the amide polymer having a fused ring structure ranges from 55% to 65%.

4. The preparation method according to claim 1, characterized in that, The graphitization process of the graphite particle precursor includes: The heating rate ranges from 2℃ / min to 5℃ / min; And / or, treat at 1300℃ to 1800℃ for 2 to 5 hours; And / or, treat at 1800℃ to 2400℃ for 2h to 5h, and hold at 2100℃ to 2200℃ for 2h; Treat at 2400℃ to 2800℃ for 2 to 5 hours; Treat at 2800°C to 3000°C for 1 to 3 hours, and then hold at 3000°C to 3100°C for 3 hours.

5. The preparation method according to claim 1, characterized in that, The solvent is one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide.

6. The preparation method according to claim 1, characterized in that, The preset mixing conditions include: a mixing temperature ranging from 25°C to 50°C, a mixing speed ranging from 500 rpm to 700 rpm, and a mixing time ranging from 10 min to 30 min. And / or, the mixing process includes one or more of fusion mixing granulation and spheroidizing mixing granulation; And / or, the coating process includes one or more of liquid phase spray coating and liquid phase fusion coating.

7. The preparation method according to claim 1, characterized in that, The preset carbonization conditions include: The protective gases used for carbonization include one or more of nitrogen or argon; The heating rate from 200°C to 600°C is 1°C / min to 2°C / min, wherein the temperature is held at 400°C to 500°C for 1 hour; and / or, the heating rate from 600°C to 1000°C is 1°C / min to 2°C / min, wherein the temperature is held at 700°C to 800°C for 1 hour; and / or, the heating rate from 1000°C to 1250°C is 1°C / min to 2°C / min, wherein the temperature is held at 1150°C to 1250°C for 2 hours.

8. The preparation method according to claim 1, characterized in that, The solvent includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide; The residual carbon content of the coating layer ranges from 0.1% to 0.5%. And / or, the attachment comprises a polymeric material having a fused ring structure, wherein the polymeric material includes , One or more of the -NH-CO- groups; in, Indicates the connection site.

9. The preparation method according to claim 8, characterized in that, The attached material includes the amide polymer having a fused ring structure.

10. A negative electrode active material, characterized in that, This includes negative electrode active materials prepared by the preparation method according to any one of claims 1 to 9.

11. The negative electrode active material according to claim 10, characterized in that, The value of D50 of the negative electrode active material ranges from 14 μm to 20 μm; And / or, the peak intensity ratio ID / IG(A) of the negative electrode active material ranges from 0.056 to 0.

108.

12. A negative electrode sheet, characterized in that, Includes the negative electrode active material as described in claim 9 or 10.

13. A secondary battery, characterized in that, Includes the negative electrode sheet as described in claim 12.

14. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 13.

Citation Information

Patent Citations

  • Lithium ion battery negative electrode material, preparation method thereof and lithium ion battery

    CN114524432A

  • Graphite composite material and preparation method and application thereof