A heat-stable polyamide wax, its preparation method and application

By introducing linear symmetrical diamines and lamellar silicate nucleating agents into polyamide waxes through synergistic design, the molecular conformation is optimized and crystal defects are targeted and sealed, thereby improving the thermal storage stability and anti-sagging performance of the coating. This solves the solvent erosion problem caused by crystal defects in existing technologies and meets the long-term protection requirements of high-end equipment.

CN121379141BActive Publication Date: 2026-11-10ZHEJIANG FENGHONG NEW MATERIAL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511648747.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-11-12
Publication Date
2026-11-10
Estimated Expiration
2045-11-12

AI Technical Summary

Technical Problem

Existing polyamide waxes suffer from crystal defects caused by the rigid steric hindrance of benzene rings during thermal storage. This allows solvents to penetrate and break down the hydrogen bond network, resulting in a decrease in coating viscosity and a collapse in anti-sagging properties, which cannot meet the long-term protection requirements of high-end equipment.

Method used

By introducing linear symmetric diamines to optimize the molecular conformation and ion-exchange bonding with lamellar silicate nucleating agents, polyamide fragments are formed, which precisely repair crystal defects and form a dynamic self-healing hydrogen bond network to block solvent penetration pathways.

Benefits of technology

It significantly improves the thermal storage stability of coatings, maintains anti-sagging properties, extends shelf life, and solves the rheological failure problem caused by crystal structure collapse in traditional technologies, making it suitable for long-term protection of high-end equipment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of rheology modifiers for coatings, and more particularly to a heat-stable polyamide wax, its preparation method, and its application. The polyamide wax comprises a polyamide wax matrix, which is formed by the condensation polymerization of an organic amine combination containing m-phenylenediamine and a linear symmetrical diamine with an acid component; and a lamellar silicate nucleating agent, the surface of which is ion-exchange bonded with polyamide fragments; the polyamide fragments are formed by the condensation of fatty acids and diamines. This invention utilizes a unique "molecular conformation optimization-defect-targeted sealing" synergistic mechanism to introduce a linear symmetrical diamine into the polyamide wax matrix, significantly reducing the inherent defect density of the crystal. Simultaneously, the lamellar silicate bonded to the polyamide fragments precisely covers residual defect sites, forming a molecular-level physical barrier that blocks solvent intrusion. This allows the coating to maintain near-initial anti-sagging properties after long-term high-temperature storage, completely solving the rheological failure problem of solvent-based coatings caused by crystal structure collapse.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating rheology modifiers, and more particularly to a heat-storage-stabilized polyamide wax, its preparation method, and its application. Background Technology

[0002] Polyamide waxes, as high-performance rheology control agents, hold an irreplaceable position in solvent-based industrial coatings. Their three-dimensional network structure formed by intermolecular hydrogen bonds effectively prevents pigment sedimentation and improves anti-sagging properties. However, semi-aromatic polyamide waxes synthesized based on m-phenylenediamine (MXDA) have significant defects: the rigid steric hindrance of the monomer benzene ring leads to an asymmetric zigzag conformation of the molecular chain, forming local lattice distortion regions during crystallization. These microscale defect sites become preferential channels for solvent molecules (such as xylene and butyl acetate) to invade, inducing the gradual disintegration of the hydrogen bond network under long-term thermal storage conditions, specifically manifested as a continuous decrease in coating viscosity and a collapse in anti-sagging properties.

[0003] Industry authoritative tests show (referencing GB / T 9264-2012) that after 60 days of accelerated aging at 60℃, the critical flow film thickness retention rate of traditional MXDA type polyamide wax is generally less than 45%, forcing downstream manufacturers to accept the industry constraint of a 6-month shelf life, which seriously restricts the long-term protection needs of high-end equipment fields such as ships and construction machinery.

[0004] To overcome the above-mentioned defects, existing technologies mainly focus on three major technical routes: metal complex systems (such as the calcium / magnesium-polyethylene oxide complex of Zhangjiagang Oasis) accelerate crystallization through ion coordination, but the migration of metal ions catalyzes the breakage of polyamide molecular chains, and obvious phase separation occurs after 120 hours of thermal aging; low molecular weight polymer nucleating agents (such as benzoic acid-terminated oligomers of Shandong Guangyin) can increase the initial crystallization temperature by 10-15℃, but the hydrogen bond matching degree between their end carboxyl groups and the polyamide backbone is insufficient, and they cannot penetrate into the interior of crystal defects. In the accelerated aging experiment, the solvent penetration rate is still as high as 68%; nanoparticle functionalization schemes (such as the TMN-22 talc system of Shanxi Chemical Research Institute) rely on heterogeneous nucleation to increase crystal density. However, the coverage of nanoparticles at defect sites is less than 25% (cryo-electron microscopy observation data), and the high surface energy leads to particle aggregation, which exacerbates local stress cracking. It is worth noting that Clariant's Licocare RBW330 and other compound systems attempt to combine lubrication and nucleation functions, but the ester bonds of the renewable wax components hydrolyze during thermal storage, causing molecular weight degradation and the release of polar small molecules, which further accelerates the solvent diffusion process.

[0005] In-depth analysis reveals fundamental limitations in existing technologies: First, there is an overemphasis on improving macroscopic crystallization rates (e.g., shortening the molding cycle by 30%) while neglecting the sealing and repair of microscopic defect structures, resulting in ineffective blocking of solvent intrusion pathways. Second, traditional nucleating agents (talc, nano-silica, etc.) lack interfacial compatibility with the polyamide matrix, leading to interfacial debonding under shear or thermal action, exposing new defect channels. Third, molecular simulations confirm that the "pocket-like" defects (approximately 1.2-2.0 nm in size) formed by the benzene ring side groups of MXDA have a specific adsorption effect on linear solvent molecules, and current technologies cannot achieve targeted sealing of these sites. Although some studies have attempted to improve dispersibility using montmorillonite or introduce fatty acid-modified interfaces, these solutions only delay rather than block solvent penetration and sacrifice more than 15% of thixotropic properties.

[0006] Therefore, developing novel modification strategies that combine defect repair capabilities with long-term thermal storage stability has become a key path to overcome the industry's technological bottlenecks. Summary of the Invention

[0007] This invention aims to overcome the shortcomings of existing technologies that generally focus on improving processing performance such as increasing crystallization rate and shortening molding cycle, while neglecting the problem of crystal structure collapse caused by solvent intrusion during thermal storage. Therefore, it provides a thermally stable polyamide wax, its preparation method, and its application to overcome the above-mentioned deficiencies.

[0008] To achieve the above-mentioned objectives, the present invention is implemented through the following technical solution: In a first aspect, the present invention provides a heat-stable polyamide wax, comprising, The polyamide wax matrix is ​​formed by the condensation polymerization of an organic amine combination containing m-phenylenediamine and a linear symmetrical diamine with an acid component; A layered silicate nucleating agent, the surface of which is bonded with polyamide segments by ion exchange; The polyamide fragment is formed by the condensation of fatty acids and diamines.

[0009] As described in the background section, this application finds that the thermal stability collapse of polyamide waxes in solvent-based coatings stems from crystal defects caused by the rigid benzene rings of m-phenylenediamine. While existing technologies have attempted to accelerate crystallization through metal complexation, increase nucleation density through low-molecular-weight polymers, or enhance physical barriers with nanoparticles, they have consistently failed to overcome two major drawbacks: first, the chemical compatibility between heterogeneous nucleating agents and the polyamide matrix is ​​insufficient, resulting in weak interfacial bonding and easy phase separation after long-term thermal storage; second, traditional nucleating agents can only increase overall crystallinity and lack selective sealing capabilities for the zigzag conformational defect sites unique to m-phenylenediamine, allowing solvent molecules to still invade along defect channels and disrupt the hydrogen bond network. This structural contradiction has led the industry to long be trapped in the problem of "improving initial rheological properties at the expense of long-term stability."

[0010] To overcome the aforementioned technical problems, this application constructs a dual synergistic mechanism of "molecular conformation optimization - defect-targeted repair". Specifically, in the design of the polyamide wax matrix, linear symmetrical diamines (such as ethylenediamine and 1,6-hexanediamine) are introduced to form a complex amine system with m-phenylenediamine. The regular molecular chains of the linear symmetrical amines can neutralize the steric hindrance effect of the benzene ring, making the molecular chains more tightly stacked, reducing the probability of crystal distortion from the source, thereby improving the crystallinity and stability of the crystal.

[0011] Furthermore, regarding the sealing of residual defects, this application abandons the traditional physical mixing or surface adsorption modification approach and effectively solves the aforementioned problems by employing a chemical bonding architecture of polyamide fragments and layered silicates. Specifically, layered silicates (such as montmorillonite) possess a unique two-dimensional topological structure, allowing their layered structure to maximize the coverage of defect sites and form a physical barrier. However, simple physical coverage cannot prevent solvent penetration along the silicate edges, nor can it form a chemical bond with the polyamide matrix. To address this, the solution designs a "molecular bridging layer" on the silicate surface, which is a polyamide fragment of a specific molecular weight bonded by ion exchange. This fragment is formed by the condensation of fatty acids and diamines, characterized by the differentiated design of its functional groups at both ends, thereby achieving stable anchoring with the silicate binding end through ionic bonds, while the exposed free amine groups (-NH2) form high-strength hydrogen bonds with the carboxyl groups of the polyamide wax matrix. This design transforms the layered silicate from a "passive filler" into an "active repair unit." In addition, the co-crystallization effect between the polyamide fragments and the matrix drives the silicate layers to preferentially migrate to the benzene ring defect region, while the amino groups at the end of the fragments effectively weave the silicate and the matrix tightly, thereby completely blocking the solvent penetration channels.

[0012] Therefore, a dynamic synergistic effect is also triggered between the material components of this application. Specifically, the matrix conformation optimized by the linear symmetric diamine significantly reduces the original defect density, while the silicate bonded to the polyamide segments can precisely repair residual defects. Moreover, the two are not simply additive: the linear amine segments in the matrix enhance the compatibility with the polyamide segments, making it easier for the silicate to embed into the lattice; and the physical barrier effect of the silicate sheets, in turn, protects the optimized molecular structure from solvent erosion. This closed-loop synergistic mechanism exhibits excellent advantages during thermal storage: the co-crystallized network of polyamide segments and matrix adaptively adjusts the hydrogen bond density with temperature changes, and even after long-term thermal cycling, the silicate sheets remain firmly anchored at the defect sites, and the solvent penetration rate is significantly suppressed. Compared with traditional nano-titanium dioxide or talc systems, which can only delay penetration for a few months, this solution achieves an improvement in the intrinsic stability of the network structure, and the coating can still maintain anti-sagging properties close to the initial state after high-temperature storage, effectively solving "shelf-life anxiety".

[0013] More importantly, this structure avoids the existing approach of treating nucleating agents as "catalysts" to accelerate crystallization. Instead, this application endows them with a novel structural repair function: by bonding polyamide fragments to the matrix at the molecular level, silicate becomes an organic extension of the polyamide crystal network, thus achieving intrinsic compatibility of heterogeneous materials at the molecular scale. Experiments demonstrate that even under strong shear or thermal shock, the silicate sheets remain firmly bonded to the matrix, without the interfacial delamination common in traditional systems.

[0014] Therefore, in summary, the technical solution in this application significantly improves thermal storage stability through the dual design of "linear symmetric diamine optimizing matrix conformation" and "polyamide fragment-bridged lamellar silicate targeted repair", while overcoming the problem of solvent-erosive collapse.

[0015] Preferably, the lamellar silicate nucleating agent accounts for 0.5-3 wt% of the polyamide wax matrix; The lamellar silicate is one of montmorillonite, mica or vermiculite, with a lamellar thickness of 10-50 nm and an aspect ratio of ≥100.

[0016] In this application, montmorillonite, mica, or vermiculite possess unique layered ion exchange capabilities, thus providing a basis for chemical bonding with polyamide fragments. Common layered minerals such as talc are excluded due to a lack of exchangeable ions. Furthermore, this application also found that excessively thin layers (<10 nm) lack sufficient mechanical strength and are prone to fracture and failure during thermal storage; excessively thick layers (>50 nm) are difficult to embed into crystal defect regions. Therefore, a layer thickness of 10-50 nm and an aspect ratio ≥100 maximizes the coverage of defect sites. A content range of 0.5-3 wt% precisely matches the defect repair requirements. Results show that below 0.5%, a continuous closed network cannot be formed, while above 3%, excessive interfacial content induces new stress concentration points.

[0017] The above-mentioned nucleating agent with specific structure adaptation achieves significant effects with a small amount of addition: its lamellar topology is oriented along the (010) crystal plane during gradient cooling to form a dense "molecular fence", which extends the penetration path of solvent molecules by several times; while the chemically bonded polyamide fragments firmly fix the lamellar to the defect site, effectively avoiding the risk of interface peeling of traditional physical mixing nucleating agents.

[0018] Preferably, the polyamide fragment has a number-average molecular weight of 800-2000 g / mol; wherein, The fatty acid is a C12-C18 straight-chain fatty acid, and the diamine is one of ethylenediamine, 1,6-hexanediamine, or p-phenylenediamine.

[0019] Preferably, the linear symmetrical diamine accounts for 8-15 wt% of the total mass of the organic amine combination, and is at least one of ethylenediamine, 1,4-butanediamine, and 1,6-hexanediamine.

[0020] The precise content (8-15 wt%) and specific type selection of linear symmetric diamines are crucial for overcoming the challenges posed by defects in m-phenylenediamine crystals. Too low a proportion of linear amine fails to effectively counteract steric hindrance, while too high a proportion disrupts the intrinsic viscosity balance of the semi-aromatic polyamide. Experiments have demonstrated that this specific combination enables the polyamide-modified silicate sheets to acquire directional driving force during gradient cooling, guiding the silicate sheets to precisely cover residual defect sites. This dynamic self-assembly effect significantly improves the targeted repair efficiency of the nucleating agent, resulting in solvent barrier effects several times greater than those of ordinary physical mixtures. More importantly, this content range avoids the rheological property degradation caused by excessive addition of traditional toughening agents, thus achieving a leap in thermal storage stability with minimal optimization.

[0021] Preferably, the acid component comprises hydroxy acids and fatty acids, with the hydroxy acids accounting for 80-90 wt% of the total mass of the acid component.

[0022] In this application, the acid component includes hydroxy acids, and the proportion of hydroxy acids is 80-90%. This proportion can precisely control the balance between hydrogen bond density and molecular chain mobility: when the hydroxy acid is less than 80%, it will lead to insufficient hydroxyl groups, resulting in a sparse hydrogen bond network, a sharp drop in the co-crystallization driving force between polyamide segments and the matrix, and difficulty in the directional migration of silicate sheets to defect sites; while when it is higher than 90%, excessive cross-linking will inhibit the conformational adjustment ability of linear symmetrical diamines, making it impossible for crystals to form "molecular guides" to guide the arrangement of sheets.

[0023] Furthermore, the polar environment provided by the hydroxy acid activates the amino group reactivity of the polyamide fragment, enabling it to dynamically repair microcracks during thermal storage, while the appropriate presence of fatty acids prevents the system from becoming excessively hydrophilic and reducing solvent barrier properties. Thus, through a three-tiered synergy with linear amine optimization and fragment bond synthesis nucleating agents, a closed-loop mechanism of "conformation optimization-targeted blocking-dynamic repair" is achieved.

[0024] Secondly, the present invention also provides a method for preparing the polyamide wax, comprising the following steps: (a) Polycondense the acid component with an organic amine until the acid value of the system drops to 15-20; (b) Add a layered silicate nucleating agent and continue the reaction until the acid value is <5; (c) After cooling, the discharged material is crushed to obtain polyamide wax.

[0025] Traditional processes either introduce nucleating agents in the early stages of polymerization, causing them to become encapsulated and ineffective by the polymer chains, or involve physical mixing in the later stages, resulting in uneven dispersion. These crude methods cannot solve the core problem of solvent penetration along crystal defects. This method creatively locks the nucleating agent addition at the mid-stage of polycondensation (acid value 15-20), when the prepolymer molecular weight is approximately 3000-5000 g / mol, forming a unique "semi-open" structure: the retained carboxyl active sites act like "molecular keyholes," allowing for precise docking with the free amine groups on the surface of the nucleating agent; while the moderate viscosity (approximately 50-200 Pa·s) provides the hydrodynamic conditions for the directional arrangement of layered silicates.

[0026] The reaction continues until the acid value is <5 after the nucleating agent is added, allowing the residual carboxyl groups to continuously condense with the amino groups of the polyamide fragments on the nucleating agent surface. This covalent bond firmly anchors the silicate sheets onto the polyamide network backbone, increasing the interfacial bonding energy several times over. Simultaneously, the gradual increase in system viscosity acts like a gentle rheological guiding force, driving the layered silicates to slide along the ordered regions of the molecular chains, ultimately forming a tile-like covering array at the benzene ring defect sites.

[0027] Preferably, after adding the lamellar silicate nucleating agent in step (b), a gradient cooling process is adopted: first, the temperature is lowered to 170-175℃ at 3-5℃ / min and held for 20-30 min, and then cooled to room temperature at 8-10℃ / min.

[0028] This application first uses a slow cooling rate of 3-5℃ / min to allow the polyamide molecular chains to fully relax above the glass transition region (170-175℃), enabling the linear symmetrical diamine to guide the molecular chains to form a regular (010) crystal orientation. Direct rapid cooling would cause the molecular chains to freeze instantly, resulting in disordered crystal planes. However, subsequent rapid cooling at 8-10℃ / min instantly freezes the optimized "silicate-matrix" composite structure, effectively avoiding the layer segregation or interface debonding caused by traditional slow cooling.

[0029] Preferably, the layered silicate nucleating agent is obtained by pretreatment through the following steps: dispersing silicate in water, adding a condensate of fatty acid and diamine, reacting at 60-80℃ for 2-4 h, and then centrifuging, drying and grinding are performed sequentially after the reaction is completed.

[0030] Thirdly, the present invention also provides the application of the polyamide wax in coatings.

[0031] Preferably, the polyamide wax is added at a rate of 0.5-3 wt% of the total mass of the coating. The coating is any one of solvent-based acrylic resin paint, epoxy resin paint, or polyurethane paint.

[0032] Therefore, this application has the following beneficial effects: This invention utilizes a unique synergistic mechanism of "molecular conformation optimization - defect-targeted sealing" to introduce linear symmetrical diamines into a polyamide wax matrix, significantly reducing the inherent defect density of the crystal. Simultaneously, it employs lamellar silicates bonded to polyamide fragments to precisely cover residual defect sites, forming a molecular-level physical barrier that blocks solvent intrusion. Combined with precise acid value control during the polycondensation process and a gradient cooling directional assembly technique, the polyamide fragments and the matrix form a dynamically self-healing hydrogen bond network, ultimately achieving a revolutionary improvement in thermal storage stability. This allows the product to maintain near-initial anti-sagging properties even after long-term high-temperature storage, completely solving the rheological failure problem caused by crystal structure collapse in solvent-based coatings, significantly extending product shelf life and expanding high-end application scenarios. Detailed Implementation

[0033] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0034] Preparation of layered silicate nucleating agents Preparation of layered silicate nucleating agent A: 100g of C36 dimer acid (Pripo l1009), 200g of stearic acid, and 65.2g of ethylenediamine were added to a reactor and reacted at 180℃ for 3h. The acid value dropped below 5, yielding a polyamide oligomer (terminated amine group) with a molecular weight of approximately 1200g / mol. 100g of sodium-based montmorillonite (layer thickness 10nm, aspect ratio 100) was dispersed in 1L of water, and 30g of the above polyamide oligomer was added. The mixture was then stirred at 80℃ for 4h to anchor the polyamide fragments between the montmorillonite layers via ionic bonds. Subsequently, 10g of ammonium stearate was added, and the mixture was treated at 70℃ for 1h. Finally, the mixture was centrifuged, dried at 110℃, and ground until D90≤5μm to obtain layered silicate nucleating agent A.

[0035] Preparation of layered silicate nucleating agent B: 80g of C36 dimer acid (Pripo l1009), 180g of lauric acid (C12), and 72g of 1,4-butanediamine were added to a reactor and polycondensed at 170℃ for 3h until the acid value reached 6.5, yielding a transparent liquid with a molecular weight of 800g / mol. Muscovite (layer thickness 50nm, aspect ratio 150) was treated with 500mL of 0.5M HCl at 60℃ for 2h to increase surface active sites. Acidified mica was dispersed in 700mL of water, and 40g of polyamide fragments were added. The mixture was emulsified under high shear at 85℃ (10000rpm) for 5h, allowing the fragments to bind through electrostatic adsorption and hydrogen bonding. Then, 20g of ammonium stearate in ethanol solution was added dropwise, and the mixture was stirred at 65℃ for 2h. Finally, the mixture was centrifuged, vacuum dried at 105℃, and ground until D90≤5μm to obtain layered silicate nucleating agent B.

[0036] Preparation of layered silicate nucleating agent C: 120g of C36 dimer acid (Pripo l1009), 160g of palmitic acid (C16) and 85g of 1,6-hexanediamine were added to a reaction vessel. The raw materials were reacted at 185℃ for 3.5h until the acid value reached 4.0, and an amber solid with a molecular weight of 2000g / mol (terminal amine content 0.50mmol / g) was obtained. 100g of expanded vermiculite (30nm thick, aspect ratio 120) was added to 600mL of aqueous solution containing 5wt% sodium citrate and sonicated (800W) for 30min. Then, 50g of polyamide fragments were added to the expanded vermiculite suspension and the temperature was increased in a stepwise manner: 60℃ / 2h → 75℃ / 2h → 90℃ / 1h, so that the interlayer spacing increased from 1.4nm to 4.2nm. Then, 25g of ammonium stearate was added and reacted at 80℃ for 1h. Finally, the mixture was centrifuged at 100℃, fluidized bed dried, and ground through an 800-mesh sieve to obtain the layered silicate nucleating agent C.

[0037] Example 1 A method for preparing a polyamide wax includes the following steps: (a) An acid component consisting of 360g of 1,2-hydroxystearic acid and 540g of sebacic acid, and an organic amine combination consisting of 368.0g of m-phenylenediamine (MXDA) and 32.0g of ethylenediamine were added to a reactor and polycondensed at 190°C for 4 hours under nitrogen protection until the acid value reached 20.0. (b) Add the above-mentioned lamellar silicate nucleating agent A5g to the system in (a) and continue the reaction at 190°C for 1h until the acid value is 4.8; (c) Cool to 175°C at 3°C / min, hold for 20 min, then cool to room temperature at 10°C / min and pulverize to obtain fine powder.

[0038] Example 2 A method for preparing a polyamide wax includes the following steps: (a) An acid component consisting of 630g of terephthalic acid and 270g of 1,2-hydroxystearic acid and an organic amine combination consisting of 340g of m-phenylenediamine and 60g of 1,6-hexanediamine were added to a reactor and polycondensed at 185°C for 5 hours under nitrogen protection until the acid value reached 15.0. (b) Add 30g of the above-mentioned lamellar silicate nucleating agent B to the system in (b), and continue the reaction at 185°C for 1.5h until the acid value is 4.2; (c) Cool to 170℃ at 5℃ / min and hold for 30 min, then cool to room temperature at 8℃ / min and pulverize to obtain micro powder.

[0039] Example 3 A method for preparing a polyamide wax includes the following steps: (a) An acid component consisting of 450g sebacic acid, 135g stearic acid, and 315g 1,2-hydroxystearic acid, and an organic amine combination consisting of 354g m-phenylenediamine (MXDA) and 46g 11,4-butanediamine were added to a reactor and polycondensed at 182°C for 4.5h under nitrogen protection until the acid value reached 17.5. (b) Add 7.5 g of the above-mentioned lamellar silicate nucleating agent C1 to the system in (b), and continue the reaction at 182 °C for 1.3 h until the acid value is 4.5; (c) Cool to 172.5℃ at 4℃ / min and hold for 25 min, then cool to room temperature at 9℃ / min and pulverize to obtain micro powder.

[0040] Example 4 A method for preparing a polyamide wax includes the following steps: (a) An acid component consisting of 585g of terephthalic acid and 315g of 1,2-hydroxystearic acid, and an organic amine combination consisting of 360g of m-phenylenediamine (MXDA) and 46g of 1,4-butanediamine were added to a reactor and polycondensed at 190°C for 4.5h under nitrogen protection until the acid value dropped to 18.5. (b) Add 15g of the above-mentioned lamellar silicate nucleating agent B1 to the system in (b), and continue the reaction at 190°C for 1.3h until the acid value is 4.3; (c) Cool to 170℃ at 5℃ / min and hold for 30 min, then cool to room temperature at 8℃ / min and pulverize to obtain micro powder.

[0041] Example 5 A method for preparing a polyamide wax includes the following steps: (a) An acid component consisting of 360g sebacic acid and 540g 1,2-hydroxystearic acid, and an organic amine combination consisting of 340g m-phenylenediamine (MXDA) and 60g 1,6-hexanediamine were added to a reactor and polycondensed at 185°C for 5.2h under nitrogen protection until the acid value dropped to 16.2. (b) The above-mentioned lamellar silicate nucleating agent C24g was added to the system in (b), and the reaction was carried out at 185°C for 1.1 h until the acid value was 4.0; (c) Cool to 175℃ at 3℃ / min and hold for 20 min, then cool to room temperature at 10℃ / min and pulverize to obtain micro powder.

[0042] Example 6 A method for preparing a polyamide wax includes the following steps: (a) An acid component consisting of 405g of terephthalic acid, 450g of 1,2-hydroxystearic acid and 45g of stearic acid, and an organic amine combination consisting of 352g of m-phenylenediamine (MXDA) and 48g of ethylenediamine were added to a reactor and polycondensed at 182°C for 4.8h under nitrogen protection until the acid value dropped to 17. (b) Add the above-mentioned lamellar silicate nucleating agent A9g to the system in (b) and react at 182°C for 1.4h until the acid value is 4.6; (c) Cool to 172℃ at 4℃ / min and hold for 25 min, then cool to room temperature at 9℃ / min and pulverize to obtain micro powder.

[0043] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 contains only 400g of m-phenylenediamine and no linear symmetrical diamines.

[0044] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the nucleating agent is unmodified sodium montmorillonite.

[0045] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that in the preparation process, a layered silicate nucleating agent is added when the polycondensation reaches an acid value of 25.0 in step (a).

[0046] Comparative Example 4 Comparative Example 4 is a commercially available competitor (Clariant Licocar RBW330).

[0047] The polyamide waxes from Examples 1-6 and Comparative Examples 1-4 were added to solvent-based acrylic resin paints at ratios of 0.5 wt% and 3 wt%, respectively. The coatings were then tested using the following methods: Thermal storage stability: According to GB / T 9264-2012 standard, the change in the thickness of the sagging film was measured after 60 days of thermal storage at 60℃ (wet film preparation device 40μm).

[0048] Solvent penetration depth: staining-cryo-electron microscopy method, adding 0.1 wt% rhodamine B dye, heat storage followed by liquid nitrogen freezing and sectioning, and confocal electron microscopy to observe the penetration depth.

[0049] Crystallinity change (ΔXc): DSC (ISO 11357), enthalpy change of fusion determined by two-stage heating method.

[0050] Thixotropic index (TI): The viscosity ratio at 6 rpm / 60 rpm was determined using a Brookfield viscometer according to ISO 2884-1.

[0051] Settling rate: Using ASTM D869, after heat storage, the top 1 / 3 of the coating was taken and the solid content change rate was measured.

[0052] The test results are shown in Table 1 and Table 2 below: Table 1. Test results of polyamide wax addition of 0.5 wt%. sample Sag retention rate (%) after 60 days Solvent penetration depth (μm) ΔXc(%) Thixotropic index (TI) before thermal storage Thixotropic index (TI) after thermal storage Settlement rate (%) Example 1 94.8 0.6 +2.9 4.1 3.9 0.7 Example 2 95.2 0.5 +3.1 4.3 4.0 0.5 Example 3 95.0 0.7 +2.8 4.0 3.8 0.8 Example 4 93.5 0.9 +2.5 3.9 3.6 1.2 Example 5 94.1 0.8 +2.7 4.2 3.9 1.0 Example 6 94.3 0.7 +2.6 4.1 3.8 0.9 Comparative Example 1 48.3 8.2 -29.6 4.0 1.8 23.5 Comparative Example 2 60.7 5.8 -20.3 4.1 2.2 17.8 Comparative Example 3 71.5 3.6 -13.2 3.9 2.8 9.4 Comparative Example 4 61.9 6.5 -23.1 4.2 2.4 19.2 Table 2. Test results of polyamide wax addition at 3wt% sample Sag retention rate (%) after 60 days Solvent penetration depth (μm) ΔXc(%) Thixotropic index (TI) before thermal storage Thixotropic index (TI) after thermal storage Settlement rate (%) Example 1 97.2 0.3 +3.5 6.5 6.3 0.2 Example 2 97.8 0.2 +3.8 6.8 6.5 0.1 Example 3 96.9 0.4 +3.2 6.3 6.0 0.3 Example 4 95.6 0.6 +2.9 6.0 5.7 0.7 Example 5 96.3 0.5 +3.1 6.4 6.1 0.5 Example 6 96.1 0.4 +3.0 6.2 5.9 0.6 Comparative Example 1 46.8 8.5 -31.2 6.5 2.1 27.3 Comparative Example 2 58.2 6.1 -22.7 6.7 2.8 21.4 Comparative Example 3 69.3 3.9 -14.6 6.1 3.3 11.8 Comparative Example 4 59.7 6.8 -25.3 6.8 2.9 23.6 The above tests on polyamide wax in solvent-based acrylic resin paints show that: At an addition rate of 0.5-3.0 wt%, the heat-stable polyamide wax in this application exhibits a sag retention rate of 93-98% and a sedimentation rate of ≤1.2% after 60 days of heat storage, indicating that its stability is superior compared to several comparative examples.

[0053] Furthermore, the crystallinity change (ΔXc) data shows that by introducing linear symmetrical diamines (such as ethylenediamine and 1,6-hexanediamine) into the structure to form a complex amine system with m-phenylenediamine, the regular molecular chains of the linear symmetrical amines can neutralize the steric hindrance effect of the benzene ring, resulting in a tighter molecular chain stacking and effectively improving crystallinity. Moreover, since this structure can reduce the probability of crystal distortion from the source, after thermal storage, the structure of the embodiment with more regular crystals remains more complete and stable. In the embodiments of this application, the crystallinity change (ΔXc) data not only did not decrease, but the crystallinity actually achieved a certain positive increase (+2.5% to +3.8%), indicating a certain self-reinforcing effect. In contrast, the comparative example, due to more lattice distortion, showed a more severe deterioration in crystallinity, resulting in a significant decrease in the crystallinity change (ΔXc) data.

[0054] Solvent penetration depth data show that, due to the adaptive adjustment of hydrogen bond density between the polyamide fragments and the matrix in this application as the temperature changes, the silicate sheets remain firmly anchored at defect sites even after long-term thermal cycling, significantly suppressing the solvent penetration rate. Therefore, within the same timeframe, the solvent penetration depth of the embodiments in this application is shallower compared to several comparative examples.

[0055] Regarding the thixotropic index (TI) data before and after heat storage, this data clearly shows the thixotropic index of acrylic resin paint containing polyamide wax before and after heat storage. The larger the difference in thixotropic index before and after heat storage, the higher its storage resistance, and thus the longer its shelf life. In several embodiments of this application, the thixotropic index fluctuation before and after heat storage is <0.5, thereby solving the shelf-life anxiety in the prior art.

[0056] In summary, the above effects stem from the synergistic effect of the optimized molecular conformation of linear symmetric diamine, the targeted sealing of crystal defects by lamellar silicate with polyamide segment bonding, the precise control of acid value during polycondensation, and the gradient cooling directional process. This effectively blocks the solvent penetration path and activates the structural self-reinforcing mechanism, enabling the coating to maintain near-initial anti-sagging properties after high-temperature storage, thus breaking through the 12-month shelf-life requirement of high-end fields.

[0057] The specific embodiments described herein are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.

Claims

1. A heat-stable polyamide wax, characterized in that, Include, The polyamide wax matrix is ​​formed by the condensation polymerization of an organic amine combination containing m-phenylenediamine and a linear symmetrical diamine with an acid component, and its acid value is 15-20 mg KOH / g. A layered silicate nucleating agent, the surface of which is bonded with polyamide segments by ion exchange; The polyamide fragment is formed by the condensation of dimer acid, fatty acid and diamine, and the number average molecular weight of the polyamide fragment is 800-2000 g / mol; The lamellar silicate is one of montmorillonite, mica, or vermiculite.

2. The polyamide wax according to claim 1, characterized in that, The layered silicate nucleating agent accounts for 0.5-3 wt% of the polyamide wax matrix; The thickness of the lamellar silicate sheets is 10-50 nm, and the aspect ratio is ≥100.

3. The polyamide wax according to claim 1, characterized in that, The fatty acid is a C12-C18 straight-chain fatty acid, and the diamine is one of ethylenediamine, 1,6-hexanediamine, or p-phenylenediamine.

4. The polyamide wax according to claim 1, characterized in that, The linear symmetrical diamine accounts for 8-15 wt% of the total mass of the organic amine combination, and is at least one of ethylenediamine, 1,4-butanediamine, and 1,6-hexanediamine.

5. The polyamide wax according to claim 1, characterized in that, The acid component comprises hydroxy acids and fatty acids, with hydroxy acids accounting for 80-90 wt% of the total mass of the acid component.

6. A method for preparing the polyamide wax according to any one of claims 1-5, characterized in that, Includes the following steps: (a) Polycondense the acid component with an organic amine until the acid value of the system drops to 15-20 mg KOH / g; (b) Add a layered silicate nucleating agent and continue the reaction until the acid value is <5 mg KOH / g; (c) After cooling, the material is crushed to obtain polyamide wax.

7. The preparation method according to claim 6, characterized in that, After adding the lamellar silicate nucleating agent in step (b), a gradient cooling process is adopted: first, the temperature is lowered to 170-175℃ at 3-5℃ / min and held for 20-30 min, and then cooled to room temperature at 8-10℃ / min.

8. The preparation method according to claim 6, characterized in that, The layered silicate nucleating agent is obtained by pretreatment through the following steps: silicate is dispersed in water, a condensate of fatty acid and diamine is added, and the mixture is reacted at 60-80℃ for 2-4 h. After the reaction is completed, the mixture is centrifuged, dried and ground in sequence.

9. The use of the polyamide wax as described in any one of claims 1-5 in coatings.

10. The application as described in claim 9, characterized in that, The amount of polyamide wax added is 0.5-3 wt% of the total mass of the coating. The coating is any one of solvent-based acrylic resin paint, epoxy resin paint, or polyurethane paint.

Citation Information

Patent Citations

  • Polyamide wax modified sericite powder and preparation method and application thereof

    CN103031015A

  • Heat storage stable polyamide wax micro powder

    CN119264720A