Infrared chalcogenide glass lens plated with M2 film as well as preparation method and application of infrared chalcogenide glass lens

By setting functional and protective layers of materials such as ZnS, Ge, YbF3, SiC and AlSi on infrared chalcogenide glass lenses, the problem of film cracking caused by stress release during DLC ​​film deposition was solved, achieving high transmittance and wear resistance, and meeting the optical performance requirements of infrared lenses.

CN121386052AInactive Publication Date: 2026-01-23FOSHAN HUAGUO OPTICAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511575553.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-31
Publication Date
2026-01-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Infrared chalcogenide glass lenses suffer from stress release issues during DLC ​​film deposition, leading to film cracking and detachment. This results in the inability to meet the spectral specifications and abrasion resistance requirements of optical thin films, as well as insufficient transmittance.

Method used

The functional and protective layers are composed of materials such as ZnS, Ge, YbF3, SiC and AlSi. An M2 film is formed on an infrared chalcogenide glass substrate through a special vapor deposition process. The film thickness and deposition conditions are optimized to ensure film adhesion and wear resistance.

Benefits of technology

It achieves an average transmittance of over 93% for infrared light in the 8-12μm range, and possesses superior wear resistance, high and low temperature resistance, solvent resistance, and water resistance, protecting the lens surface and meeting the optical thin film spectral specifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121386052A_ABST
    Figure CN121386052A_ABST
Patent Text Reader

Abstract

The invention relates to an infrared chalcogenide glass lens plated with an M2 film in the technical field of infrared optical materials, the infrared chalcogenide glass lens comprises an infrared chalcogenide glass substrate, and a functional layer and a protective layer which are plated on the infrared chalcogenide glass substrate in sequence, and the functional layer comprises at least one ZnS layer, at least one YbF3 layer, at least one Ge layer and at least one SIC layer; the functional layer and the protective layer are arranged on the infrared chalcogenide glass substrate, the ZnS layer, the Ge layer, the YbF3 layer and the SIC layer are used as the functional layer, the AlSi layer and the polysiloxane layer are used as the protective layer, and the components of the functional layer and the protective layer are selected, so that the prepared infrared chalcogenide glass lens is good in film color black-like uniformity, high in reproducibility, high in light transmittance and high in light transmittance. According to the present invention, the infrared glass lens prepared by using the method can meet the requirement that the average transmittance of the infrared ray of 8-12 [mu] m is greater than 93%, the actually measured average transmittance is greater than 93.95%, and the infrared glass lens has characteristics of strong wear resistance, high and low temperature resistance, solvent etching resistance and water immersion resistance, and can provide effects of infrared glass lens surface protection, solvent etching resistance and rain and sewage water seepage prevention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of infrared optical materials technology, and in particular to an infrared chalcogenide glass lens coated with an M2 film, its preparation method, and its application. Background Technology

[0002] Germanium (Ge), a high-quality infrared material, is a non-renewable rare metal and is subject to national control. Considering the cost and development of infrared lens products, it is necessary to optimize the design from a technical perspective and replace germanium lenses with other infrared materials to reduce costs and enhance product competitiveness. The ideal solution is to replace germanium lenses with infrared chalcogenide glass lenses as a technological innovation.

[0003] To replace germanium lenses with infrared chalcogenide glass lenses, a thin film meeting the spectral requirements needs to be deposited on the surface of the infrared chalcogenide glass using a vapor deposition process. The strength of this infrared film must be similar to that of DLC (dichlorodimethyl sulfide) film. The resulting film must withstand over 10,000 abrasion cycles under a force of 1 kg / cm². This abrasion-resistant film ultimately protects the surface of the infrared glass lens, preventing solvent corrosion and water seepage. Furthermore, the film color must closely resemble the black color of DLC film, as per customer requirements. Conventional DLC films offer strong abrasion resistance and effectively protect the lens surface; however… Unlike Ge or Si materials, infrared chalcogenide glass is a non-conductive material. During the DLC film deposition process, the film in infrared chalcogenide lenses fails to release stress effectively. Finished lenses coated with DLC films on infrared chalcogenide glass often suffer from poor quality due to film cracking and detachment during stress release. This problem is not easily detected, and DLC can only achieve a transmittance of about 91% for 8-12 μm. Therefore, coating chalcogenide glass with DLC films is an ideal alternative to non-chalcogenide glass. To this end, we propose an infrared chalcogenide glass lens coated with M2 film, its preparation method, and its application.

[0004] Existing technologies for infrared chalcogenide glass lenses cannot conventionally deposit DLC films to meet the spectral requirements of infrared optical films, the quality requirements for protecting the first element of the lens, and the requirement for a black film appearance. Only through unconventional deposition methods can the design of infrared chalcogenide lenses achieve the required optical film spectral transmittance. This involves designing a special M2 film system using special materials with varying thicknesses and under specific deposition conditions. This approach achieves the required spectral transmittance of the infrared chalcogenide glass lens while simultaneously achieving a single-pass infrared lens with a transmittance of 1 kg / cm². 2 The M2 film, which has withstood more than 10,000 abrasions under pressure, exhibits excellent and stable reproducibility in terms of spectral transmittance and film quality with each deposition. Summary of the Invention

[0005] To address the aforementioned problems, this invention provides an infrared chalcogenide glass lens coated with an M2 film, its preparation method, and its application. By selecting the components of the functional layer and the protective layer, the resulting infrared chalcogenide glass lens exhibits good near-black uniformity, strong reproducibility, and meets the requirement of an average transmittance of infrared light at 8-12μm greater than 93%. Furthermore, it possesses superior wear resistance, high and low temperature resistance, solvent corrosion resistance, and water immersion resistance.

[0006] The technical solution of this invention is: An infrared chalcogenide glass lens coated with an M2 film includes an infrared chalcogenide glass substrate and a functional layer and a protective layer sequentially disposed on the infrared chalcogenide glass substrate. The functional layer includes at least one ZnS layer, at least one YbF3 layer, at least one Ge layer and at least one SiC layer, and the protective layer includes an AlSi layer and a polysiloxane layer.

[0007] In a further technical solution, the functional layers, from the inside out, are the first ZnS layer, the first Ge layer, the first YbF3 layer, the first SiC layer, the second ZnS layer, the second Ge layer, and the third ZnS layer.

[0008] In a further technical solution, the AlSi layer and the polysiloxane layer in the protective layer are arranged sequentially from the inside to the outside.

[0009] In a further technical solution, the thickness of the first ZnS layer is 500 to 700 nm; the thickness of the second ZnS layer is 80 to 200 nm; and the thickness of the third ZnS layer is 80 to 200 nm.

[0010] In a further technical solution, the thickness of the first Ge layer is 30 to 120 nm, and the thickness of the first Ge layer is 80 to 180 nm.

[0011] In a further technical solution, the thickness of the YbF3 layer is 700 to 1400 nm.

[0012] In a further technical solution, the thickness of the SiC layer is 60 to 200 nm; the thickness of the AlSi layer is 40 to 150 nm; and the thickness of the polysiloxane layer is 5 to 40 nm.

[0013] The present invention also claims protection for a method for preparing an infrared chalcogenide glass lens coated with an M2 film, comprising the following steps: placing an infrared chalcogenide glass substrate in a coating machine, and sequentially depositing the functional layer and the protective layer on the surface of the glass substrate to obtain the infrared chalcogenide glass lens coated with an M2 film and appearing black.

[0014] The present invention also claims protection for the application of the infrared chalcogenide glass lens coated with the M2 film in an infrared thermal imager.

[0015] The present invention also claims protection for an infrared thermal imager comprising an infrared chalcogenide glass lens coated with the aforementioned M2 film.

[0016] The beneficial effects of this invention are: This invention sets functional layers and protective layers on an infrared chalcogenide glass substrate. ZnS, Ge, YbF3, and SiC layers are used as functional layers, while AlSi and polysiloxane layers are used as protective layers. By selecting the components of the functional and protective layers, the resulting infrared chalcogenide glass lens exhibits good uniformity in black color, strong reproducibility, and meets the requirement of an average transmittance of over 93% for infrared light at 8-12 μm (measured average transmittance greater than 93.95%). Furthermore, it possesses strong wear resistance, high and low temperature resistance, solvent corrosion resistance, and water immersion resistance, thus protecting the surface of the infrared glass lens and providing protection against solvent corrosion, rain, and water seepage. Attached Figure Description

[0017] Figure 1 This is a design curve diagram of the special membrane system M2 in an embodiment of the present invention; Figure 2 This is a graph showing the average transmittance of the M2 membrane in an embodiment of the present invention. Detailed Implementation

[0018] The embodiments of the present invention will be further described below with reference to the accompanying drawings.

[0019] In the following examples and comparative examples, the SiC film (silicon carbide compound material) has a refractive index of 2.69 at 550 nm; the AlSi film (aluminum-silicon compound material) has a refractive index of 1.48 at 550 nm; the CHSiOx (polysiloxane) film has a refractive index of 1.46 at 550 nm; and the Ge, ZnS, and YbF3 layers are common optical film materials in the art. Unless otherwise specified, other raw materials, reagents, or devices used in the following examples or comparative examples can be obtained from conventional commercial sources or by existing known methods. Example

[0020] An infrared chalcogenide glass lens coated with an M2 film includes an infrared chalcogenide glass substrate and a functional layer and a protective layer sequentially disposed on the infrared chalcogenide glass substrate. The functional layer comprises, from the inside out, a first ZnS layer with a thickness of 580 nm, a first Ge layer with a thickness of 80 nm, a second ZnS layer with a thickness of 120 nm, a second Ge layer with a thickness of 125 nm, a third ZnS layer with a thickness of 180 nm, and a first YbF3 layer with a thickness of 1145 nm. The protective layer comprises, from the inside out, a SiC layer with a thickness of 150 nm, an AlSi layer with a thickness of 80 nm, and a polysiloxane layer (CHSiOx) with a thickness of 15 nm.

[0021] A method for preparing an infrared chalcogenide glass lens coated with an M2 film includes the following steps: The infrared chalcogenide glass substrate to be coated is placed in an AR vapor deposition machine, and the vacuum pressure is kept below 3 × 10⁻⁶. -4 After baking at 220℃ for 60 min, the lens was cleaned with an argon ion source for 30 min. Then, the following layers were deposited sequentially on the lens surface using molybdenum boat resistive evaporation and electron gun evaporation: a first ZnS layer with a thickness of 580 nm, a first Ge layer with a thickness of 80 nm, a second ZnS layer with a thickness of 120 nm, a second Ge layer with a thickness of 125 nm, a third ZnS layer with a thickness of 180 nm, a first YbF3 layer with a thickness of 1145 nm, and a first SiC layer with a thickness of 135 nm. The protective layer consisted of an AlSi layer with a thickness of 80 nm and a polysiloxane layer (CHSiOx) with a thickness of 15 nm from the inside out. After the evaporation was completed, the lens was baked at 220℃ for 60 min and then cooled for 120 min to obtain an infrared chalcogenide glass lens with M2 film. Example

[0022] An infrared chalcogenide glass lens coated with an M2 film includes an infrared chalcogenide glass lens and a functional layer and a protective layer sequentially disposed on the infrared chalcogenide glass lens. The functional layer comprises, from the inside out, a first ZnS layer with a thickness of 648 nm, a first Ge layer with a thickness of 93 nm, a second ZnS layer with a thickness of 105 nm, a second Ge layer with a thickness of 112 nm, a third ZnS layer with a thickness of 150 nm, a first YbF3 layer with a thickness of 1025 nm, and a first SiC layer with a thickness of 115 nm. The protective layer comprises, from the inside out, an AlSi layer with a thickness of 120 nm and a polysiloxane layer (CHSiOx) with a thickness of 25 nm.

[0023] A method for preparing an infrared chalcogenide glass lens coated with an M2 film includes the following steps: The infrared chalcogenide glass lens to be coated is placed in an AR vapor deposition coating machine, and the vacuum pressure is kept below 3×10⁻⁶. -4After baking at 250℃ for 60 min, the lens was cleaned with an argon ion source for 30 min. Then, the following layers were sequentially deposited on the lens surface using molybdenum boat resistive evaporation and electron gun evaporation: a first ZnS layer with a thickness of 648 nm, a first Ge layer with a thickness of 93 nm, a second ZnS layer with a thickness of 105 nm, a second Ge layer with a thickness of 112 nm, a third ZnS layer with a thickness of 150 nm, a first YbF3 layer with a thickness of 1025 nm, and a first SiC layer with a thickness of 115 nm. The protective layer consisted of an AlSi layer with a thickness of 120 nm and a polysiloxane layer (CHSiOx) with a thickness of 25 nm, from the inside out. After evaporation, the lens was baked at 250℃ for 60 min and then cooled for 120 min. The infrared chalcogenide glass lens with M2 film was obtained. Example

[0024] An infrared chalcogenide glass lens coated with an M2 film includes an infrared chalcogenide glass lens and a functional layer and a protective layer sequentially disposed on the infrared chalcogenide glass lens. The functional layer comprises, from the inside out, a first ZnS layer with a thickness of 642 nm, a first Ge layer with a thickness of 48 nm, a second ZnS layer with a thickness of 121 nm, a second Ge layer with a thickness of 118 nm, a third ZnS layer with a thickness of 112 nm, a first YbF3 layer with a thickness of 965 nm, and a first SiC layer with a thickness of 102 nm. The protective layer comprises, from the inside out, an AlSi layer with a thickness of 100 nm and a polysiloxane layer (CHSiOx) with a thickness of 28 nm.

[0025] A method for preparing an infrared chalcogenide glass lens coated with an M2 film includes the following steps: The infrared chalcogenide glass lens to be coated is placed in an AR vapor deposition coating machine, and the vacuum pressure is kept below 3×10⁻⁶. -4 After baking at 180℃ for 60 min, the lens was cleaned with an argon ion source for 30 min. Then, the following layers were sequentially deposited on the lens surface using molybdenum boat resistive evaporation and electron gun evaporation: a first ZnS layer with a thickness of 642 nm, a first Ge layer with a thickness of 48 nm, a second ZnS layer with a thickness of 121 nm, a second Ge layer with a thickness of 118 nm, a third ZnS layer with a thickness of 112 nm, a first YbF3 layer with a thickness of 965 nm, and a first SiC layer with a thickness of 102 nm. The protective layer consisted of an AlSi layer with a thickness of 100 nm and a polysiloxane layer (CHSiOx) with a thickness of 28 nm, from the inside out. After evaporation, the lens was baked at 180℃ for 60 min and then cooled for 120 min. The infrared chalcogenide glass lens with M2 film was obtained.

[0026] Due to the requirements of infrared thin film optical spectral specifications, the thickness of the vapor-deposited film can be relatively thick when different film materials are combined. Furthermore, chalcogenide glass is subject to significant stress during optical thin film deposition, resulting in poor film adhesion, susceptibility to film detachment and cracking, and weak abrasion resistance. Therefore, it is crucial to carefully set and test relevant conditions to improve and eliminate film stress and enhance the abrasion resistance of the M2 film. A dedicated infrared coating vapor deposition machine was used to optimize and test various coating conditions; the design and trial development of M2 film with different film material combinations were realized. Technical solutions adopted to solve technical problems: The stress improvement condition setting test is shown in the table below: Lens surface cleaning Argon ion source purge for 10-30 minutes Baking temperature before vapor deposition 100~250℃ Baking time before vapor deposition 50~120 minutes Baking temperature after vapor deposition 100~250℃ Baking time after vapor deposition 50~120 minutes Cooling temperature after vapor deposition 50~100℃ Infrared optical thin film spectral transmission specifications require the design of the top few layers to be coated with a special film system consisting of a specific compound AlSi+CHSiOX combined with an ultra-strong protective film layer, and coating experiments, development and testing are conducted. The special membrane system design for M2 membranes is shown in the table below: membrane material Ge ZnS Ge ZnS <![CDATA[YbF3]]> ZnS SIC AlSi CHSIOX Film thickness(nm) 52 645 116 102 924 108 113 120 30 like Figure 1 The figure shown is a design curve of the special membrane system M2.

[0027] Through repeated trial coating tests under different conditions, the M2 film infrared chalcogenide glass lens that meets the requirements was finally successfully coated. The specific environmental test results of the M2 film are as follows: Testing methods Test conditions Test Results Results Explanation determination Membrane strength test Apply 2cm wide 3M tape with a peel strength of not less than 2.7N / cm to the surface of the film layer, lift it vertically and repeatedly 3 times, then wipe the surface clean and inspect it. The quality of the coating on a reflective visual inspection lens under an 11W desk lamp. Visual reflection inspection after testing: no film peeling on the film surface. OK Temperature test A constant temperature and humidity test chamber was used to maintain the temperature at -62±2℃ and +70±2℃ for 2 hours each, during which the rate of temperature change must not exceed 2℃ / min. The membrane was inspected at room temperature (16 to 32°C). No defects such as delamination or cracks were found, indicating it was OK. Finally, MC610 test tape was applied to the membrane surface and quickly pulled vertically. No delamination was observed, indicating it was OK. Visual reflection inspection after environmental testing: no film detachment; MC610 test tape was quickly pulled up without film detachment. OK Damp heat test A constant temperature and humidity test chamber was used to maintain the temperature at 50±2℃ and relative humidity at 95% to 100% for 24 hours. The film layer is free from problems such as peeling, delamination, cracking, and fading. Visual reflection inspection after environmental testing: The film layer showed no problems such as peeling, delamination, cracks, or fading. OK Temperature shock test The temperature was maintained at (-40±2)℃ for 30 minutes, then increased to (85±2)℃ at a rate of 5℃ / min, and stabilized for 30 minutes as one cycle, for a total of 24 cycles. The quality of the coating on a reflective visual inspection lens under an 11W desk lamp. Visual reflection inspection after environmental testing: No abnormalities such as peeling, delamination, cracks, or blistering were found in the film. OK Solvent resistance and wipe test Using a soaking solution box, immerse the product in trichloroethylene, acetone, and anhydrous ethanol for 10 minutes each, and then wipe it with a degreased cloth for inspection. The film surface is free from problems such as delamination, scratches, and fading. Visual reflection inspection after environmental testing: The film layer showed no problems such as peeling, delamination, cracks, or fading. OK Boiling water test Using a rice cooker, boil water to 100 degrees Celsius, then place the sulfur-based material sheet coated with M2 film into the boiling water and boil continuously for 24 hours. No membrane delamination or bubbles, OK. Visual reflection inspection after environmental testing: no film delamination or bubbles were found in the film layer. OK Abrasion resistance test A wear-resistant wiping machine was used, with a rubber head wrapped in 6 layers of degreased cloth, and a force of 1KG was applied to rub the film surface along the same trajectory for testing. After 10,000+ cycles of continuous rubbing, the film surface showed no damage or delamination, which is good. Visual reflection inspection after environmental testing: After 10,000+ cycles of continuous rubbing, there were no scratches or delamination on the film surface. OK Salt spray test Salt spray testing was used, with the temperature of the salt spray test chamber set at 35±2℃, the salt spray solution concentration at 4% to 6%, the pH value at 6.5 to 7.2, and the duration at 504 hours. No defects such as membrane peeling or flaking in the membrane layer, OK. Visual reflection inspection after environmental testing: No defects such as membrane peeling or flaking were found in the membrane layer. OK As can be seen from the table above, the infrared chalcogenide glass lens coated with M2 film of the present invention passed the high and low temperature cycling test, damp heat test, solvent resistance test, boiling water test, abrasion resistance test of 10,000+ cycles, and salt spray test.

[0028] like Figure 2 As shown, the average transmittance curve of the M2 membrane spectrum requires: 8-12um Tave ≥ 93%, and the actual measured result is 93.95%.

[0029] The above embodiments merely illustrate specific implementations of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention.

Claims

1. An infrared chalcogenide glass lens plated with a M2 film, characterized in that, The infrared chalcogenide glass substrate and the functional layer and the protective layer which are sequentially arranged on the infrared chalcogenide glass substrate, the functional layer comprises at least one ZnS layer, at least one YbF3 layer, at least one Ge layer and at least one SIC layer, and the protective layer comprises an AlSi layer and a polysiloxane layer.

2. The infrared chalcogenide glass ophthalmic lens coated with a M2 film according to claim 1, characterized in that: The functional layer comprises a first ZnS layer, a first Ge layer, a first YbF3 layer, a first SIC layer, a second ZnS layer, a second Ge layer and a third ZnS layer from inside to outside.

3. The infrared chalcogenide glass ophthalmic lens coated with a M2 film according to claim 1, wherein: The AlSi layer and the polysiloxane layer in the protective layer are sequentially arranged from inside to outside.

4. The infrared chalcogenide glass ophthalmic lens coated with a M2 film according to claim 2, wherein: The thickness of the first ZnS layer is 500-700 nm, the thickness of the second ZnS layer is 80-200 nm, and the thickness of the third ZnS layer is 80-200 nm.

5. The infrared chalcogenide glass ophthalmic lens coated with a M2 film according to claim 2, wherein: The thickness of the first Ge layer is 30-120 nm, and the thickness of the second Ge layer is 80-180 nm.

6. The infrared chalcogenide glass ophthalmic lens coated with a M2 film according to claim 2, wherein: The thickness of the YbF3 layer is 700-1400 nm.

7. The infrared chalcogenide glass ophthalmic lens coated with a M2 film according to claim 2, wherein: The thickness of the SIC layer is 60-200 nm, the thickness of the AlSi layer is 40-150 nm, and the thickness of the polysiloxane layer is 5-40 nm.

8. The method of claim 1-7, wherein the method further comprises, The method comprises the following steps: placing an infrared chalcogenide glass substrate in a coating machine, and sequentially evaporating the functional layer and the protective layer on the surface of the glass substrate to obtain the infrared chalcogenide glass lens coated with the M2 film.

9. The infrared chalcogenide glass lens coated with the M2 film according to any one of claims 1-7 is used in an infrared thermal imager.

10. An infrared thermal imager characterized by, The infrared chalcogenide glass lens coated with the M2 film according to any one of claims 1-7.